Optimization of Precision Casting Process for Engine Cylinder Block Components

This study investigates the optimization of precision casting parameters for critical engine cylinder block components using numerical simulation and experimental validation. Through systematic analysis of process variables, we demonstrate significant improvements in defect reduction and production efficiency.

Engine cylinder block casting process

1. Material Characteristics and Thermal Analysis

The engine cylinder block components utilize 4Cr9Si2 martensitic heat-resistant steel with the following thermal properties:

$$ \lambda(T) = 28.5 + 0.012T \quad [W/m·K] $$
$$ H(T) = 850 + 0.6T \quad [kJ/kg] $$

Where $\lambda$ represents thermal conductivity and $H$ denotes enthalpy. The temperature-dependent characteristics significantly influence solidification behavior and defect formation.

2. Process Parameter Optimization

Three critical parameters were identified for engine cylinder block casting optimization:

Parameter Level 1 Level 2 Level 3
Pouring Temperature (°C) 1570 1600 1630
Pouring Time (s) 3 4 5
Shell Preheat (°C) 1050 1100 1150

The orthogonal test results revealed the following optimal combination for engine cylinder block production:

Test A B C Defect Rate (%)
1 1570 3 1050 1.724
2 1570 4 1100 1.572
3 1570 5 1150 1.953
4 1600 3 1100 1.629
5 1600 4 1150 1.897
6 1600 5 1050 1.483
7 1630 3 1150 2.060
8 1630 4 1050 1.513
9 1630 5 1100 1.367

3. Statistical Analysis of Process Parameters

The significance of parameters on engine cylinder block quality was determined through ANOVA:

$$ R_A = 0.310 $$
$$ R_B = 0.611 $$
$$ R_C = 1.342 $$

Factor Sum of Squares F-value Significance
Shell Preheat 0.360 114.08 Most Significant
Pouring Time 0.066 20.80 Significant
Temperature 0.018 5.60 Not Significant

4. Solidification Dynamics

The critical solid fraction for effective feeding in engine cylinder block casting is defined as:

$$ f_s^{critical} = 70\% $$

Simulation results demonstrate that optimized parameters achieve sequential solidification from component to gating system, ensuring adequate liquid metal feeding throughout the process.

5. Production Validation

Implementation of the optimized parameters (1630°C pouring temperature, 5s filling time, 1100°C shell preheat) yielded:

  • Defect rate reduction from 3.358% to 1.367%
  • Qualification rate improvement from 50% to 91.67%
  • Elimination of surface pits and shrinkage cavities

This systematic approach provides a reliable methodology for precision casting of complex engine cylinder block components, with direct applications in automotive and aerospace manufacturing.