I have applied a low-melting alloy fusible pattern method to sand mould casting for a closed aluminum alloy impeller with fifteen blades and a highly complex flow path. The impeller was narrow in its internal passages, mostly non-machined on the flow surfaces, and severely twisted in blade geometry. In my experience, a conventional sand mould casting route using separately assembled sand cores produces an excessive accumulation of positional and dimensional errors. Those errors become especially dangerous when the final wall thickness is only about one millimeter and when the core itself must be about seven millimeters thick. I therefore developed an integral core-making method in which the blade patterns are made from a fusible alloy, assembled in the core box, embedded in core sand, and then melted out during baking. This approach preserved the advantages of sand mould casting while greatly improving flow-channel dimensional accuracy and surface finish.

From the first trials, I recognized that the main difficulty was not the external shape of the impeller but the internal core that forms the fifteen flow passages. If the core is made as a set of small separate pieces, each piece must be positioned, glued, vented, and supported. Every interface adds a tolerance. In sand mould casting, those tolerances can shift during ramming, handling, baking, and pouring. The final result is often a flow passage that is locally too narrow or too wide, and a blade that is thinner than the minimum allowed. Because the impeller must run with very low unbalance, even a small deviation in blade position can create vibration and dynamic-balance problems. The fusible pattern method removes most of those interfaces by making the entire flow-passage core in one piece.
Geometry and Process Demands
I began by quantifying the impeller geometry. The small end of the impeller had fifteen double-curved blades distributed on a circle with a diameter of about fifty millimeters. The minimum gap between adjacent blades was only about six and a half millimeters. The blade angle to the base plate changed smoothly from about thirty-one degrees thirty minutes to ninety degrees, and the blade twist was large. After machining, two wall sections were only about one millimeter thick. This meant that the core forming the seven-millimeter flow channel had to be positioned within a very tight envelope. On a diameter of about two hundred eighty millimeters, the allowable deviation of the core was no more than about half a millimeter. Otherwise the casting would suffer from missing metal, or “short run,” and would be scrapped.
| Parameter | Value or Range | Impact on Sand Mould Casting |
|---|---|---|
| Number of blades | 15 | Requires equal angular spacing and identical blade profiles |
| Small-end blade circle diameter | 50 mm | Sets the tightest angular and radial tolerance zone |
| Minimum blade gap | 6.5 mm | Limits core sand thickness and core strength |
| Blade-to-base angle | 31°30′ to 90° | Creates severe twist and prevents rigid pattern withdrawal |
| Flow-channel core thickness | 7 mm | Requires high core dimensional stability |
| Finished wall thickness after machining | 1 mm at two locations | Any core shift can cause missing metal |
| Outlet diameter | 280 mm | Amplifies angular and radial deviations |
| Permissible core deviation on 280 mm diameter | ≤0.5 mm | Defines the target accuracy for sand mould casting |
| Unbalance eccentricity requirement | <1 μm | Demands accurate blade position and mass distribution |
| Casting material | Al-Si-Mg cast alloy, T6 condition | Requires controlled cooling and feeding |
| Net casting mass | 4 kg | Affects pouring time and solidification modulus |
| Machining allowance | 4 mm | Provides limited compensation for distortion |
I used the following relations to evaluate the blade spacing and flow area. The angular pitch for fifteen blades is fixed:
$$\theta_p = \frac{360^\circ}{N} = \frac{360^\circ}{15} = 24^\circ$$
The chord spacing at the small-end diameter is approximately:
$$s = D_p \sin\left(\frac{\theta_p}{2}\right) = 50 \sin(12^\circ) \approx 10.4 \text{ mm}$$
If the local blade thickness is about 3.9 mm, the minimum gap becomes:
$$g_{\min} = s – t_b \approx 10.4 – 3.9 = 6.5 \text{ mm}$$
The flow area of one passage can be expressed as an integral over the radial coordinate:
$$A_f = \int_{r_1}^{r_2} \left[ \frac{2\pi r}{N} – t_b(r) \right] dr$$
These equations showed me that the core cross-section was small and that any angular misalignment would directly reduce the local flow area. In sand mould casting, the core must therefore be made as a single, dimensionally stable body. The statistical tolerance stack for an assembled core is:
$$T_{asm} = \sqrt{\sum_{i=1}^{n} T_i^2}$$
For an integral core, the number of independent tolerance contributors is drastically reduced. The arithmetic worst-case stack is:
$$T_{asm} = \sum_{i=1}^{n} T_i$$
By moving from many assembled pieces to one fusible-pattern core, I reduced the dimensional chain from many links to essentially one. This is the central reason why the sand mould casting process became viable for this impeller.
Why Integral Core Making Was Necessary
I compared several possible core-making routes before committing to the fusible pattern method. The traditional route is to make each blade passage with a separate sand core, then assemble the cores in the mould. This is common in sand mould casting, but it requires many joints. Each joint can shift during handling and pouring. The second route is to use a collapsible or soluble core, but the materials available to me did not offer the needed strength and thermal stability. The third route is the one I selected: a low-melting alloy fusible pattern that is embedded in the core sand and later melted out. This creates an integral sand core with the exact external shape of all fifteen passages.
| Core-Making Route | Number of Core Pieces | Typical Deviation Risk | Suitability for This Impeller |
|---|---|---|---|
| Separately assembled sand cores | 15 or more | High cumulative error at joints | Not suitable |
| Collapsible metal core | 1 or several | Limited by extraction and clearance | Not suitable for severe twist |
| Soluble or washout core | 1 | Dependent on material strength and removal | Possible but not selected |
| Fusible alloy pattern integral core | 1 | Low, because pattern is cast and checked before coring | Selected and proven |
In my trials, the integral core made by the fusible pattern method gave the best balance of accuracy, surface quality, and manufacturability. It also allowed me to inspect and weigh each fusible pattern before it was embedded in sand. That step is very important for sand mould casting, because it lets me reject a bad pattern before it becomes a bad core.
Low-Melting Alloy Selection
I needed an alloy that would melt and flow out of the core during baking, without damaging the core sand. I tested alloys with melting temperatures from about sixty to two hundred degrees Celsius. The results showed a clear window. If the melting temperature was too high, the core tended to spall or lose pieces. If the melting temperature was too low, the core deformed during handling or baking. The best results came from a four-element alloy based on bismuth, tin, lead, and cadmium, with a melting temperature of about one hundred fifty degrees Celsius, controlled within plus or minus five degrees.
| Alloy Melting Temperature | Observed Core-Making Result | Decision |
|---|---|---|
| Above 200 °C | Core sand easily breaks away; edges spall | Rejected |
| 150 ± 5 °C | Core quality good; clean melt-out; stable shape | Selected |
| Below 100 °C | Core deforms easily; poor handling strength | Rejected |
The alloy composition must be controlled because small changes in bismuth, tin, lead, and cadmium shift the melting range. I used the following approximate roles for the elements. The exact charge was adjusted by melting-point measurement before production.
| Element | Role in the Fusible Alloy | Approximate Mass Fraction Range |
|---|---|---|
| Bismuth | Lowers melting point; controls solidification range | 40–60% |
| Tin | Improves fluidity and castability | 5–20% |
| Lead | Adjusts melting point; reduces cost | 20–40% |
| Cadmium | Narrows melting range; improves pattern detail | 5–15% |
The liquidus temperature of a multicomponent alloy can be approximated by a mixing rule with a eutectic depression term:
$$T_m \approx \sum_i x_i T_{m,i} – \Delta T_{mix}$$
For my selected alloy, the target was:
$$T_m = 150 \pm 5^\circ C$$
This temperature was chosen because it matched the core-baking schedule. It was high enough to keep the pattern rigid during core ramming, yet low enough to melt out completely before the core reached its final cure temperature. In sand mould casting, this balance is critical because the core must survive handling and metal pouring, but the pattern must disappear without leaving residue that would create gas defects.
Manufacturing the Fusible Pattern
I produced the fusible patterns by two methods. For trial work and single-piece production, I used sand mould casting of the fusible alloy. For repeatable production, I used a simple metal mould. Both methods worked, but the metal mould gave better surface finish, better dimensional consistency, and better weight control. The sand mould casting route for the fusible pattern was faster for a new design because no metal tooling was required. The metal mould route was better once the blade geometry was fixed.
| Pattern Manufacturing Route | Advantages | Limitations | Best Use |
|---|---|---|---|
| Sand mould casting of fusible alloy | Short lead time; low tooling cost; easy changes | More hand finishing; less repeatable | Prototype and single-piece work |
| Metal mould casting of fusible alloy | Good surface; high dimensional accuracy; consistent weight | Requires metal tooling; higher initial cost | Small-to-medium batch production |
For the metal mould process, I controlled the mould temperature and the alloy pouring temperature. If the mould was too cold, the fusible pattern filled poorly. If the mould was too hot, the pattern cooled slowly and shrank inconsistently. The following parameters gave me the best results.
| Parameter | Value | Effect |
|---|---|---|
| Metal mould working temperature | 60–100 °C | Improves fill and reduces thermal shock |
| Alloy pouring temperature for metal mould | 235 ± 5 °C | Ensures complete fill without excessive shrinkage |
| Alloy pouring temperature for sand mould | 190 ± 10 °C | Suits lower heat extraction of sand |
| Pattern weight tolerance | ±3 g | Controls mass distribution of the final impeller |
The pattern shrinkage can be estimated from:
$$L_m = L_p (1 + \alpha_p \Delta T)$$
where $$L_m$$ is the mould cavity dimension, $$L_p$$ is the required pattern dimension, $$\alpha_p$$ is the thermal contraction coefficient of the fusible alloy, and $$\Delta T$$ is the temperature difference. I used this relation to compensate the metal mould cavity. I also checked every pattern by weight:
$$\Delta W = W_i – W_{ref}, \quad |\Delta W| \le 3 \text{ g}$$
The relative weight deviation is:
$$\delta_W = \frac{|\Delta W|}{W_{ref}} \times 100\%$$
This weight check is a simple but powerful quality gate. In sand mould casting of a dynamically balanced impeller, a small mass error in one blade can shift the center of gravity. By weighing each fusible pattern, I ensured that the final cast impeller had a consistent mass distribution before the metal was ever poured.
Core Sand Formulation and Baking
The core sand had to be strong enough to survive handling and pouring, yet porous enough to allow the melted alloy to flow out. I used a quartz sand base with tung oil, bentonite, dextrin, and water. The tung oil provided green strength and baked strength. Bentonite improved plasticity. Dextrin helped the core surface finish. The formulation I used is shown below.
| Component | Mass Fraction | Function |
|---|---|---|
| Quartz sand, 70–140 mesh | 100% | Refractory base; controls surface finish |
| Tung oil | 2.0–2.3% | Binder; develops baked strength |
| Bentonite | 1.5% | Plasticity and green strength |
| Dextrin | 1.0% | Surface finish and collapsibility |
| Water | As needed | Tempering and molding |
I prepared the core by assembling the fusible patterns in the core box, filling the box with core sand, and ramming it carefully around the narrow blade passages. After ramming, I removed the top half of the core box and placed the core, still supported by the bottom half, into an electric furnace. The furnace temperature was raised until the fusible alloy melted and flowed out of the core. Then I removed the bottom half and baked the core again to develop full strength. After cooling to room temperature, I lightly dressed the core and placed it into the sand mould.
| Stage | Temperature | Purpose | Control Point |
|---|---|---|---|
| Melt-out stage | 150–200 °C | Melt and drain the fusible alloy | Alloy must flow freely; no trapped pockets |
| Initial bake | 180–220 °C | Develop handling strength | Avoid rapid heating that can crack the core |
| Final bake | 220–250 °C | Cure the binder and remove volatiles | Uniform temperature; adequate ventilation |
| Cooling | Ambient | Stabilize core dimensions | Cool in dry, clean environment |
The heat required to melt out the pattern can be estimated by:
$$Q = m_p [c_s (T_m – T_0) + L_f + c_l (T_b – T_m)]$$
where $$m_p$$ is the mass of the fusible pattern, $$c_s$$ is the solid specific heat, $$L_f$$ is the latent heat of fusion, $$c_l$$ is the liquid specific heat, $$T_0$$ is room temperature, $$T_m$$ is the melting point, and $$T_b$$ is the baking temperature. I used this estimate to ensure that the furnace schedule supplied enough heat to melt the alloy completely without overheating the core sand. In sand mould casting, incomplete melt-out is a serious defect because residual alloy becomes a gas source or a hard inclusion inside the core.
Sand Mould Casting Practice
After the integral core was ready, I placed it in the sand mould and closed the mould. The moulding sand was a conventional clay-bonded sand suitable for aluminum alloy casting. I paid special attention to core support and venting because the flow passages were narrow. The core had to be located accurately in the mould, but it also had to be vented so that gases could escape during pouring. If the core is over-constrained, it may crack. If it is under-supported, it may shift. I used a combination of core prints, chaplets, and controlled clearances to achieve the required position.
For the gating system, I used a bottom-fill or stepped gating arrangement to reduce turbulence. Aluminum alloys are sensitive to oxide films and gas entrapment. A smooth, non-turbulent fill is important in sand mould casting of thin-wall impellers. I also used a riser or feeding path to compensate for solidification shrinkage. The solidification modulus of the casting can be estimated by:
$$M = \frac{V}{A}$$
where $$V$$ is the volume of the casting section and $$A$$ is its cooling surface area. For the thick sections near the hub and the outer rim, I increased the feeding efficiency by using a larger modulus riser or a chill. For the thin blade sections, I relied on the high cooling rate of the sand mould to produce fine grains and good strength.
The pouring time can be approximated by:
$$t_f = K \sqrt{G}$$
where $$G$$ is the casting mass and $$K$$ is an empirical coefficient that depends on the alloy and mould condition. In my sand mould casting trials, I adjusted the pouring time to avoid cold shuts in the blade tips and to avoid sand erosion in the gating system. The combination of a fusible-pattern integral core and controlled sand mould casting gave a complete fill in all fifteen passages.
| Casting Variable | Approach I Used | Reason |
|---|---|---|
| Mould material | Clay-bonded sand | Compatible with existing sand mould casting line |
| Gating | Bottom-fill or stepped | Reduces turbulence and oxide entrapment |
| Core support | Core prints and controlled clearance | Prevents shift without cracking |
| Venting | Core vents and mould vents | Removes gases from binder and alloy |
| Feeding | Riser and chills where needed | Compensates shrinkage in thick sections |
| Pouring temperature | Adjusted for Al-Si-Mg alloy | Balances fluidity and gas absorption |
Dimensional Accuracy and Surface Finish
The most important improvement I observed was in the outlet width of the impeller and the parallelism of the two surfaces that form that width. Over the full diameter of about two hundred eighty millimeters, the deviation in outlet width and parallelism was no greater than half a millimeter. This was far better than the normal sand mould casting tolerance for this type of casting. The flow passages were smooth and free from the steps and ridges that often occur when assembled cores shift. The surface finish of the flow path was also significantly improved, which reduced the need for manual polishing and helped the impeller meet its dynamic-balance requirement.
| Quality Characteristic | Conventional Sand Mould Casting with Assembled Cores | My Fusible Pattern Integral Core Sand Mould Casting |
|---|---|---|
| Number of core pieces per impeller | 15 or more | 1 |
| Outlet width deviation on 280 mm diameter | Usually greater than 1.0 mm | ≤0.5 mm |
| Parallelism of outlet surfaces | Variable; often out of tolerance | ≤0.5 mm |
| Flow-passage surface finish | Rough; joint lines and fins | Smooth; no joint lines |
| Risk of missing metal at thin walls | High | Greatly reduced |
| Dynamic balance | Difficult to achieve | Consistently achievable |
| Scrap rate in my trials | High | All parts accepted |
The dimensional improvement can be understood through the tolerance equations. For an assembled core, the total radial deviation at the blade tip is approximately:
$$T_{radial} = \sum_{i=1}^{n} T_i + T_{assembly}$$
For the integral core, the assembly term is eliminated, leaving only the pattern tolerance, core shrinkage, and mould location:
$$T_{radial} \approx T_{pattern} + T_{core} + T_{mould}$$
Because I could inspect and weigh each fusible pattern, I held $$T_{pattern}$$ very small. The core shrinkage was controlled by the sand formulation and baking schedule. The mould location was controlled by the core prints and moulding practice. The result was a total radial deviation within the half-millimeter requirement. This is why the fusible pattern method was so effective in sand mould casting for this impeller.
Defect Prevention and Process Control
I encountered several potential defects during development and developed controls for each one. The most common risks were incomplete melt-out, core deformation, gas holes, and shrinkage porosity. Incomplete melt-out usually came from a pattern that was too large in cross-section or from a baking schedule that was too slow. Core deformation came from handling the core while it was still hot or from insufficient binder. Gas holes came from residual alloy, binder volatiles, or poor venting. Shrinkage porosity came from inadequate feeding in the hub and rim.
| Defect | Probable Cause | Control I Applied |
|---|---|---|
| Incomplete melt-out | Low baking temperature; trapped alloy | Raise melt-out stage; provide drain paths; verify pattern weight |
| Core deformation | Weak binder; hot handling; uneven baking | Increase tung oil within range; cool before handling; uniform furnace load |
| Gas holes | Residual alloy; poor venting; wet sand | Complete melt-out; add core vents; control water content |
| Shrinkage porosity | Insufficient feeding; thick sections | Increase riser modulus; use chills; adjust pouring temperature |
| Blade misalignment | Pattern shift in core box | Check pattern fit; use locating features; weigh and inspect each pattern |
| Sand burn-on | High pouring temperature; reactive sand | Control pouring temperature; use suitable coating; improve sand quality |
| Cold shut | Low pouring temperature; slow fill | Adjust gating; increase pour temperature; reduce heat loss |
For gas-related defects, I used a simple venting criterion. The vent area should be large enough to allow the gas generated during pouring to escape without raising the internal pressure above the metal static pressure. In practice, I increased the number of core vents and ensured that each vent communicated with the mould atmosphere. This is a standard precaution in sand mould casting, but it becomes even more important when the core is made by a fusible pattern method because any residual alloy can generate gas.
Production Experience and Results
I moved the process from trial to production after confirming that the integral core could be made repeatedly. In the first production campaign, I cast eight impellers in two heats. All of them were accepted. In a later campaign, I cast five more impellers with the same method, and again all were accepted. The user later requested additional parts, which confirmed that the process was stable and reliable. The combination of low-melting alloy fusible patterns and sand mould casting gave a robust route for a component that would otherwise have required a much more expensive casting method or extensive machining.
| Production Run | Number of Impellers | Accepted | Rejected | Qualification Rate |
|---|---|---|---|---|
| First trial campaign | 8 | 8 | 0 | 100% |
| Second production campaign | 5 | 5 | 0 | 100% |
| Follow-up order | Additional parts | Accepted | 0 | 100% in my records |
The economic benefit came from several sources. First, the scrap rate fell dramatically because the thin walls no longer suffered from missing metal. Second, the surface finish of the flow passages improved, which reduced the time required for manual finishing and polishing. Third, the integral core eliminated the labor needed to assemble and glue many small cores. Fourth, the weight control on the fusible patterns reduced the need for correction balancing after machining. These factors made the fusible pattern method competitive even though the low-melting alloy and the metal pattern tooling added some cost.
| Cost or Benefit Factor | Effect of Fusible Pattern Integral Core |
|---|---|
| Core assembly labor | Eliminated |
| Core dimensional scrap | Reduced to near zero |
| Flow-passage finishing | Reduced because surface is smoother |
| Dynamic balancing | Easier because blade mass is consistent |
| Tooling cost | Higher if metal mould is used, but amortized over batch |
| Pattern material cost | Recovered and reused where practical |
| Overall scrap rate | Greatly reduced |
Key Process Parameters and Formulas
For anyone applying this method to sand mould casting, I recommend documenting the key parameters and checking them before every production run. The fusible alloy melting point, pattern weight, core sand formulation, baking schedule, and pouring conditions are all critical. The following summary table collects the most important values from my work.
| Parameter | Recommended Value or Range |
|---|---|
| Fusible alloy melting point | 150 ± 5 °C |
| Alloy system | Bi-Sn-Pb-Cd four-element alloy |
| Metal mould working temperature | 60–100 °C |
| Alloy pouring temperature into metal mould | 235 ± 5 °C |
| Alloy pouring temperature into sand mould | 190 ± 10 °C |
| Pattern weight tolerance | ±3 g |
| Core sand base | Quartz sand, 70–140 mesh |
| Tung oil addition | 2.0–2.3% |
| Bentonite addition | 1.5% |
| Dextrin addition | 1.0% |
| Melt-out temperature | 150–200 °C |
| Final bake temperature | 220–250 °C |
| Maximum core deviation on 280 mm diameter | ≤0.5 mm |
The main dimensional relations I used were:
$$\theta_p = \frac{360^\circ}{N}$$
$$s = D_p \sin\left(\frac{\theta_p}{2}\right)$$
$$g_{\min} = s – t_b$$
$$A_f = \int_{r_1}^{r_2} \left[ \frac{2\pi r}{N} – t_b(r) \right] dr$$
$$T_{asm} = \sqrt{\sum_{i=1}^{n} T_i^2}$$
$$T_{radial} \approx T_{pattern} + T_{core} + T_{mould}$$
$$L_m = L_p (1 + \alpha_p \Delta T)$$
$$\Delta W = W_i – W_{ref}$$
$$\delta_W = \frac{|\Delta W|}{W_{ref}} \times 100\%$$
$$Q = m_p [c_s (T_m – T_0) + L_f + c_l (T_b – T_m)]$$
$$M = \frac{V}{A}$$
$$t_f = K \sqrt{G}$$
These equations are not a substitute for shop-floor trials, but they helped me set the initial parameters and understand why the integral core worked so well. In sand mould casting, small changes in core position can have a large effect on the final impeller. By controlling the pattern, the core, and the mould as three separate but linked systems, I was able to hold the final dimensions within the required tolerance.
Comparison with Conventional Sand Mould Casting
It is useful to state clearly how the fusible pattern method changes the conventional sand mould casting approach. In conventional sand mould casting, the core is usually made from sand and then assembled inside the mould. The core pieces must be strong enough to handle, and they must be located accurately. Each piece has its own tolerance. The assembly process adds another tolerance. When the metal is poured, the core may shift because of buoyancy, erosion, or thermal expansion. The final casting reflects all of these errors.
In my method, the fusible pattern becomes the core. The pattern is made first, inspected, and weighed. It is then embedded in core sand. The sand takes the shape of the pattern. When the pattern melts out, the sand core retains that shape. There is no assembly of many small pieces. There is no glue line. There is no cumulative tolerance stack from fifteen separate cores. This is the fundamental reason why the fusible pattern method improves sand mould casting accuracy for this type of impeller.
| Feature | Conventional Sand Mould Casting | Fusible Pattern Sand Mould Casting |
|---|---|---|
| Core construction | Multiple sand pieces assembled | One integral sand core formed around fusible patterns |
| Dimensional chain | Long; many joints | Short; pattern and core dominate |
| Surface finish of passages | Joint lines, fins, steps | Smooth, continuous surfaces |
| Blade position accuracy | Difficult to maintain | Controlled by pattern and core box |
| Thin-wall integrity | High risk of missing metal | Low risk when core is centered |
| Dynamic balance | Harder to achieve | Easier because mass distribution is controlled |
| Process complexity | Simple materials, complex assembly | Special alloy, simpler core assembly |
Practical Recommendations
Based on my experience, I recommend the following practices for applying a fusible pattern to sand mould casting of complex impellers. First, select the alloy melting point to match the core-baking schedule. A melting point of about one hundred fifty degrees Celsius worked best for me. Second, use a metal mould for the fusible pattern whenever production volume justifies it. The metal mould gives better surface finish and weight consistency. Third, weigh every fusible pattern and reject any that exceeds the weight tolerance. This is one of the cheapest and most effective quality controls. Fourth, design the core box with adequate locating features so that the fusible patterns cannot shift during ramming. Fifth, provide sufficient vents in the core and mould. Sixth, control the baking schedule carefully. A slow, uniform heating cycle prevents core cracking and ensures complete melt-out. Seventh, verify the core dimensions before closing the mould. A simple check of the outlet width and blade spacing can prevent a costly scrap.
I also recommend recording the following data for each production lot: alloy melting point, pattern weight, core sand batch, baking temperature and time, pouring temperature, pouring time, and final inspection results. With this data, it is possible to trace any variation back to its source. In sand mould casting, traceability is often the difference between a stable process and a mysterious scrap problem.
Conclusion
I have shown that a low-melting alloy fusible pattern can be used to make an integral core for sand mould casting of a closed aluminum alloy impeller with fifteen blades and a complex flow path. The method replaces a large number of assembled sand cores with a single core formed around a cast fusible pattern. The pattern is melted out during baking, leaving a clean and accurate core cavity. The resulting sand mould casting has better flow-channel dimensional accuracy, better surface finish, and better dynamic-balance potential than conventional sand mould casting with assembled cores.
The key parameters are a fusible alloy melting point of about one hundred fifty degrees Celsius, a pattern weight tolerance of plus or minus three grams, a core sand formulation based on quartz sand with tung oil, bentonite, and dextrin, and a controlled baking schedule that completely melts and drains the alloy before final cure. The dimensional target of no more than half a millimeter deviation on a two hundred eighty millimeter diameter was achieved. Production trials gave a one hundred percent qualification rate in my records. For complex impeller castings, this fusible pattern integral core method is a practical and reliable extension of sand mould casting technology.