In this work I investigated the numerical simulation and process optimization of a machine tool slide seat produced by sand mould casting. The slide seat is a critical moving component in a machine tool. It supports the worktable, transmits cutting forces, and guides precision motion. Because the part has a long, ribbed, variable-section geometry, the conventional trial-and-error method for sand mould casting is slow, expensive, and highly dependent on expert experience. I therefore combined casting simulation, gating system comparison, chill and riser design, additive and subtractive mould manufacturing, and orthogonal process parameter optimization to improve casting quality and shorten the production cycle.

1. Research Motivation and Objectives
Sand mould casting remains the dominant route for producing machine tool castings because it offers good formability, low cost, and wide material adaptability. However, for a slide seat with large overall dimensions and non-uniform wall thickness, sand mould casting often produces shrinkage porosity, residual stress, and deformation. These defects reduce stiffness, damping, and service life. Traditional sand mould casting optimization relies on repeated trial pours. Each trial requires a long mould-making cycle, high mould modification cost, and significant manual labor. The problem becomes more severe for single-piece and small-batch production, where the mould cost cannot be amortized over many parts.
My main objectives were therefore:
1. To analyze the slide seat structure and select a suitable cast iron material for sand mould casting.
2. To design top, parting, and bottom gating systems and compare their filling, solidification, and shrinkage porosity behavior.
3. To optimize the selected sand mould casting process by adding chills, insulating risers, and vents.
4. To manufacture the upper and lower sand moulds using additive and subtractive methods instead of conventional pattern-based moulding.
5. To optimize pouring temperature, pouring time, and sand mould preheating temperature using an orthogonal experiment.
2. Casting Process Design for Sand Mould Casting
2.1 Structure and Material
The slide seat has an envelope size of approximately \(1510\,\text{mm} \times 445\,\text{mm} \times 516\,\text{mm}\). Its net weight is about \(305.68\,\text{kg}\). The maximum wall thickness is about \(45\,\text{mm}\), and the minimum wall thickness is about \(18\,\text{mm}\). Most of the body has a relatively uniform wall thickness near \(18\,\text{mm}\), but local thick sections create hot spots during sand mould casting. I selected HT250 gray cast iron because it balances strength, wear resistance, damping capacity, and cost. HT250 is widely used for high-load machine tool parts. Its low melting point, good fluidity, and small shrinkage make it suitable for sand mould casting.
| Property or Element | Value or Range |
|---|---|
| Material | HT250 gray cast iron |
| Tensile strength | \(\geq 250\,\text{MPa}\) |
| C | 3.16–3.30 wt% |
| Si | 1.79–1.93 wt% |
| Mn | 0.89–1.04 wt% |
| S | 0.094–0.125 wt% |
| P | 0.120–0.170 wt% |
2.2 Casting Design Parameters
For sand mould casting, the pattern dimensions must compensate for solidification shrinkage. The casting shrinkage \(K\) is defined as
$$K = \frac{L_M – L_J}{L_J} \times 100\%$$
where \(L_M\) is the pattern dimension and \(L_J\) is the casting dimension. For small and medium gray iron castings, I used a free shrinkage of about \(1.0\%\) and a restrained shrinkage of about \(0.9\%\). Considering the slide seat geometry, I selected a shrinkage of \(1.0\%\).
| Gray Iron Type | Free Shrinkage (%) | Restrained Shrinkage (%) |
|---|---|---|
| Small and medium | 1.0 | 0.9 |
| Medium and large | 0.9 | 0.8 |
| Extra large | 0.8 | 0.7 |
I also applied a machining allowance of about \(2\,\text{mm}\) to the surfaces that require machining. For minimum cast holes, I used the following rule: for single-piece and small-batch gray iron castings, holes smaller than about \(50\,\text{mm}\) are usually left for machining, while larger holes may be cast directly. This reduces machining time and avoids unnecessary hot spots in sand mould casting.
| Production Batch | Minimum Cast Hole Diameter for Gray Iron (mm) |
|---|---|
| Large batch | 12–15 |
| Medium batch | 15–30 |
| Single piece and small batch | 30–50 |
2.3 Gating System Design
The gating system controls metal flow, filling time, slag entrapment, gas entrainment, and thermal distribution. In sand mould casting, an improper gating system can cause cold shuts, misruns, sand erosion, gas porosity, and shrinkage defects. I designed three gating systems according to the position of the ingate: a top gating system, a parting gating system, and a bottom gating system.
| Gating System | Ingate Position | Main Advantages | Main Risks |
|---|---|---|---|
| Top gating | Top of the casting | Easy filling, favorable for directional solidification | Metal splash, oxidation, gas entrainment, sand erosion |
| Parting gating | Middle height, on parting plane | Stable filling, simple moulding, balanced thermal field | Requires careful ingate design |
| Bottom gating | Bottom of the casting | Very stable filling, low turbulence, good gas escape | Low top temperature, unfavorable for riser feeding |
I modeled all three gating systems in a 3D CAD environment. A pouring basin and sprue well were included to reduce metal impact and stabilize flow. The slide seat had an important machined surface that had to be protected from shrinkage porosity. I therefore compared the three designs through numerical simulation before selecting the final sand mould casting layout.
2.4 Pouring Parameters
The pouring temperature affects fluidity, shrinkage, gas absorption, and mould reaction. For HT250, I used the relationship between wall thickness and pouring temperature shown below. Because the main wall thickness of the slide seat is about \(18\,\text{mm}\), I selected a pouring temperature range of \(1370\text{–}1440^\circ\text{C}\).
| Material | Main Wall Thickness (mm) | Pouring Temperature (\(^\circ\text{C}\)) |
|---|---|---|
| HT250 | 8–15 | 1390–1450 |
| HT250 | 15–30 | 1370–1440 |
| HT250 | 30–50 | 1350–1430 |
| HT250 | >50 | 1270–1360 |
The pouring time \(t\) was calculated using the empirical formula for gray iron:
$$t = S_1 \sqrt[3]{\delta G}$$
where \(\delta\) is the main wall thickness in mm, \(G\) is the pouring weight in kg including the gating and riser system, and \(S_1\) is a coefficient. For this slide seat, \(G \approx 452.7\,\text{kg}\), \(\delta = 45\,\text{mm}\), and \(S_1 = 1.2\). This gave a pouring time of about \(24\,\text{s}\). I checked the result using the liquid surface rise velocity:
$$v = \frac{h}{t}$$
where \(h\) is the casting height during pouring. With \(h = 288\,\text{mm}\) and \(t = 24\,\text{s}\), the rise velocity was \(12\,\text{mm/s}\). The allowable minimum rise velocity for gray iron with wall thickness between 10 and 40 mm is about \(10\text{–}20\,\text{mm/s}\), so the pouring time was acceptable.
I also calculated the sand mould preheating temperature from the empirical relation
$$T_{\text{mould}} = \frac{1}{3} T_{\text{pour}} \pm T_{\text{corr}}$$
where \(T_{\text{pour}}\) is the pouring temperature and \(T_{\text{corr}}\) is a correction coefficient. For metal mould casting, \(T_{\text{corr}}\) is often taken as \(30^\circ\text{C}\). Applying this relation to the selected pouring temperature range gave a sand mould preheating temperature range of \(430\text{–}510^\circ\text{C}\). Preheating reduces the chilling effect, improves metal fluidity, and helps gas escape, but excessive preheating slows solidification and may reduce mechanical properties.
3. Numerical Simulation Theory for Sand Mould Casting
I used a finite element based casting simulation package to model the sand mould casting process. The simulation considered filling, solidification, shrinkage porosity, residual stress, and deformation. The governing equations are summarized below.
3.1 Filling and Flow Model
Molten metal was treated as an incompressible Newtonian fluid. The mass conservation equation is
$$\frac{\partial \rho}{\partial t} + \frac{\partial(\rho u_x)}{\partial x} + \frac{\partial(\rho v_y)}{\partial y} + \frac{\partial(\rho w_z)}{\partial z} = 0$$
For incompressible flow, this becomes
$$\frac{\partial u_x}{\partial x} + \frac{\partial v_y}{\partial y} + \frac{\partial w_z}{\partial z} = 0$$
The momentum conservation equations are
$$\rho \left( \frac{\partial u_x}{\partial t} + u_x \frac{\partial u_x}{\partial x} + v_y \frac{\partial u_x}{\partial y} + w_z \frac{\partial u_x}{\partial z} \right) = -\frac{\partial p}{\partial x} + \rho g_x + \mu \nabla^2 u_x$$
$$\rho \left( \frac{\partial v_y}{\partial t} + u_x \frac{\partial v_y}{\partial x} + v_y \frac{\partial v_y}{\partial y} + w_z \frac{\partial v_y}{\partial z} \right) = -\frac{\partial p}{\partial y} + \rho g_y + \mu \nabla^2 v_y$$
$$\rho \left( \frac{\partial w_z}{\partial t} + u_x \frac{\partial w_z}{\partial x} + v_y \frac{\partial w_z}{\partial y} + w_z \frac{\partial w_z}{\partial z} \right) = -\frac{\partial p}{\partial z} + \rho g_z + \mu \nabla^2 w_z$$
The energy conservation equation is
$$\rho c \left( \frac{\partial T}{\partial t} + u_x \frac{\partial T}{\partial x} + v_y \frac{\partial T}{\partial y} + w_z \frac{\partial T}{\partial z} \right) = \frac{\partial}{\partial x}\left( k \frac{\partial T}{\partial x} \right) + \frac{\partial}{\partial y}\left( k \frac{\partial T}{\partial y} \right) + \frac{\partial}{\partial z}\left( k \frac{\partial T}{\partial z} \right) + S$$
The volume of fluid function \(F\) is used to track the free surface:
$$\frac{\partial F}{\partial t} + u_x \frac{\partial F}{\partial x} + v_y \frac{\partial F}{\partial y} + w_z \frac{\partial F}{\partial z} = 0$$
3.2 Solidification Model
During solidification, heat transfer is dominated by conduction between the metal and the sand mould, convection between the mould and air, and radiation from exposed surfaces. The conduction equation is
$$\rho c \frac{\partial T}{\partial t} = \frac{\partial}{\partial x}\left( \lambda \frac{\partial T}{\partial x} \right) + \frac{\partial}{\partial y}\left( \lambda \frac{\partial T}{\partial y} \right) + \frac{\partial}{\partial z}\left( \lambda \frac{\partial T}{\partial z} \right) + Q$$
Convection is described by Newton’s law of cooling:
$$q = \alpha (T_f – T_w)$$
Radiation follows the Stefan–Boltzmann law:
$$E = \varepsilon \sigma_0 T_s^4$$
where \(\sigma_0 = 5.67 \times 10^{-8}\,\text{W}/(\text{m}^2 \cdot \text{K}^4)\).
3.3 Shrinkage Porosity Criteria
For shrinkage porosity prediction, I used the POROS criterion available in the simulation software. This criterion is suitable for gravity sand mould casting and considers both microporosity and macroporosity. The Niyama criterion is also widely used:
$$\frac{G}{\sqrt{R}} < C_{\text{Niyama}}$$
where \(G\) is the local temperature gradient, \(R\) is the cooling rate, and \(C_{\text{Niyama}}\) is a critical value. However, because the Niyama criterion was originally developed for steel castings, I relied on the POROS model for the gray iron slide seat. In the POROS model, regions with a porosity value greater than \(0.01\) are considered macroporosity, while smaller values indicate dispersed microporosity.
3.4 Stress and Deformation Model
I used an elastic–plastic model to calculate thermal stress and deformation. The elastic stress–strain relation is
$$\sigma = D_e \varepsilon_e$$
The von Mises equivalent stress is
$$\sigma_{\text{eq}} = \sqrt{\frac{1}{2}\left[(\sigma_1-\sigma_2)^2 + (\sigma_2-\sigma_3)^2 + (\sigma_3-\sigma_1)^2\right]}$$
The total strain is decomposed as
$$\varepsilon = \varepsilon_e + \varepsilon_p + \varepsilon_t$$
The thermal strain increment is
$$d\varepsilon_t = \left( \alpha dT + \frac{\partial \alpha}{\partial T}(T-T_0)dT \right)$$
These equations allowed me to predict residual stress and deformation after sand mould casting.
4. Simulation of the Three Gating Systems
I imported the three gating system models into the simulation software, generated surface and volume meshes, and assigned material properties. The casting and gating system used a finer mesh, while the sand box used a coarser mesh. The main simulation settings are listed below.
| Parameter | Setting |
|---|---|
| Gravity direction | Vertical downward, \(9.8\,\text{m/s}^2\) |
| Metal material | HT250 |
| Mould material | Resin sand |
| Chill material | Steel |
| Pouring temperature | \(1380^\circ\text{C}\) |
| Pouring time | \(24\,\text{s}\) |
| Sand mould preheating temperature | \(450^\circ\text{C}\) |
| Casting–mould heat transfer coefficient | \(500\,\text{W}/(\text{m}^2\cdot\text{K})\) |
| Casting–chill heat transfer coefficient | \(2000\,\text{W}/(\text{m}^2\cdot\text{K})\) |
| Mould–chill heat transfer coefficient | \(500\,\text{W}/(\text{m}^2\cdot\text{K})\) |
| External boundary condition | Air cooling, \(T = 20^\circ\text{C}\) |
4.1 Filling Behavior
For the top gating system, metal entered from the top and fell into the mould cavity. The filling process was generally stable, but there was slight splashing and erosion in the early stage. This could cause sand inclusion, gas entrainment, or surface defects in sand mould casting.
For the parting gating system, metal entered from the middle height. The flow velocity was appropriate, and no obvious splashing or erosion occurred. The cavity filled smoothly from the bottom toward the top. The liquid surface rose uniformly, and the filling process met the requirements of sand mould casting.
For the bottom gating system, metal entered from the bottom and filled the cavity from bottom to top. The flow was very stable and no splashing occurred. However, the bottom region remained hot for a long time, which delayed solidification and reduced the feeding efficiency of the risers.
4.2 Solidification Behavior
In all three gating systems, thin walls solidified first, while thick sections solidified later. The bottom thick sections and the important machined surface were the last regions to solidify. Because these regions did not receive sufficient liquid metal feeding, they became hot spots and formed shrinkage porosity. The bottom gating system had the slowest solidification because the bottom metal remained superheated for a longer time.
4.3 Shrinkage Porosity Prediction
I compared the predicted shrinkage porosity volume for the three gating systems. The results are summarized below.
| Gating System | Shrinkage Porosity Volume (\(\text{cm}^3\)) | Filling Stability | Solidification Behavior |
|---|---|---|---|
| Top gating | 147.20 | Moderate, slight splashing | Favorable top-to-bottom gradient |
| Parting gating | 132.58 | Good, stable | Balanced thermal field |
| Bottom gating | 136.43 | Very good, very stable | Slow bottom cooling, poor riser feeding |
The parting gating system produced the smallest shrinkage porosity volume and the most stable filling behavior. I therefore selected the parting gating system as the basis for further optimization in sand mould casting.
5. Process Optimization of the Selected Sand Mould Casting Design
The simulation showed that the thick sections and the important machined surface still suffered from shrinkage porosity. To solve this problem, I added chills, insulating risers, and vents. Chills accelerate cooling in thick sections and reduce hot spots. Insulating risers provide liquid metal feeding to the last solidifying regions. Vents allow gas to escape from the mould cavity and reduce gas porosity.
5.1 Chill Design
I placed steel chills with thicknesses between \(10\,\text{mm}\) and \(15\,\text{mm}\) on the thick wall regions that were prone to hot spots. The chills increased the local cooling rate and promoted directional solidification toward the risers. This reduced the temperature gradient between the thick and thin sections.
5.2 Riser Design
I placed four insulating risers on the important machined surface. These risers remained liquid longer than the casting and provided feeding metal to the hot spots. They also helped collect slag and gas. The risers were positioned so that the last solidification occurred inside the riser rather than in the casting.
5.3 Vent Design
I added vents at the high points of the mould cavity. During filling and solidification, air and binder decomposition gases can be trapped if venting is insufficient. The vents reduced gas pressure and helped prevent blowholes, gas porosity, and backpressure defects in sand mould casting.
5.4 Optimized Simulation Results
After adding chills, risers, and vents, I reran the simulation. The filling process remained stable. The solidification sequence became more directional: thin walls solidified first, thick walls solidified next, and the risers solidified last. The shrinkage porosity volume decreased from \(132.58\,\text{cm}^3\) to \(1.42\,\text{cm}^3\). Residual stress and deformation were also predicted.
| Item | Before Optimization | After Optimization |
|---|---|---|
| Shrinkage porosity volume (\(\text{cm}^3\)) | 132.58 | 1.42 |
| Residual stress (MPa) | Not specifically optimized | 1351.1 |
| Deformation (mm) | Not specifically optimized | 2.32 |
The optimized sand mould casting process greatly reduced the risk of shrinkage porosity. The remaining porosity was small and dispersed, which is acceptable for the service requirements of the slide seat.
6. Mould Manufacturing by Additive and Subtractive Methods
Traditional sand mould casting requires a pattern, a core box, and a moulding process. For single-piece and small-batch production, pattern making is time-consuming and expensive. I therefore used a hybrid additive–subtractive route. The upper sand mould was produced by 3D sand printing, while the lower sand mould was produced by CNC milling. This approach shortened the mould manufacturing cycle and reduced trial-and-error cost.
6.1 Equipment
For additive manufacturing, I used a large-scale sand printer with a working envelope of \(2000\,\text{mm} \times 1000\,\text{mm} \times 800\,\text{mm}\). The system included a sand mixing unit, a precision sand printing unit, and a sand screening unit. For subtractive manufacturing, I used a digital patternless casting precision forming machine with a working envelope of \(3000\,\text{mm} \times 1500\,\text{mm} \times 900\,\text{mm}\). The machine included a CNC software system, a movable platform, and a pneumatic system.
6.2 Sand Material Selection
I selected silica sand as the base material because it is inexpensive, refractory, chemically stable, and widely used in sand mould casting. I compared three sand samples by particle size distribution. The standard sample had the smallest average particle size and the most concentrated distribution. A finer sand provides more contact area with resin, faster curing, higher density, and more binder bridges. Therefore, I selected the standard silica sand with a grain size of \(70/140\) mesh.
| Particle Size (\(\mu\text{m}\)) | Standard Sample (%) | Sample 1 (%) | Sample 2 (%) |
|---|---|---|---|
| 75 | 0.25 | 0.11 | 0 |
| 100 | 1.26 | 0.64 | 0.05 |
| 200 | 39.98 | 29.89 | 4.50 |
| 300 | 86.22 | 73.52 | 31.43 |
| 400 | 98.79 | 93.36 | 68.13 |
| 500 | 99.96 | 98.85 | 89.63 |
| 600 | 100 | 99.91 | 97.89 |
For the binder system, I used a furan resin, a mixed sulfonic acid curing agent, and a cleaning agent. The resin has low viscosity, high strength, fast curing, and low harmful emissions. The curing agent has good fluidity and low corrosion. The cleaning agent is used to clean the printhead and dissolve residual resin.
| Material | Typical Property | Value |
|---|---|---|
| Furan resin | Density at \(20^\circ\text{C}\) | \(1.10\text{–}1.20\,\text{g/cm}^3\) |
| Furan resin | Viscosity at \(20^\circ\text{C}\) | \(13.5\text{–}17.0\,\text{mPa}\cdot\text{s}\) |
| Curing agent | Density at \(20^\circ\text{C}\) | \(1.20\text{–}1.30\,\text{g/cm}^3\) |
| Curing agent | Viscosity at \(20^\circ\text{C}\) | \(\leq 20\,\text{mPa}\cdot\text{s}\) |
| Cleaning agent | Viscosity at \(20^\circ\text{C}\) | \(\leq 10\,\text{mPa}\cdot\text{s}\) |
6.3 Sand Sample Performance Tests
I printed standard sand specimens and tested tensile strength, compressive strength, shear strength, permeability, and gas evolution. The results are shown below.
| Test | Measured Average | Requirement |
|---|---|---|
| Tensile strength | \(2.465\,\text{MPa}\) | > \(1.5\,\text{MPa}\) |
| Compressive strength | \(4.093\,\text{MPa}\) | > \(3.5\,\text{MPa}\) |
| Shear strength | \(1.820\,\text{MPa}\) | > \(1.5\,\text{MPa}\) |
| Permeability | \(160.8\) | \(\approx 160\) |
| Gas evolution | \(10\,\text{mL/g}\) | < \(12\,\text{mL/g}\) |
The printed sand met the required strength, permeability, and gas evolution values. Therefore, the selected sand and binder system were suitable for sand mould casting of the slide seat.
6.4 Mould Partitioning
I designed the mould parting based on the gating system and the capabilities of the additive and subtractive machines. The sand mould size was approximately \(1780\,\text{mm} \times 765\,\text{mm} \times 389\,\text{mm}\). I used a vertical parting design with an upper sand mould and a lower sand mould. The region below the runner was placed in the lower mould, and the region above the runner was placed in the upper mould. Cores were used for internal cavities and holes to maintain dimensional accuracy and reduce the number of mould pieces.
6.5 Upper Mould by 3D Sand Printing
I imported the upper mould model into a 3D printing preparation software, positioned it within the build box, and sliced it into layers. The layer thickness was \(0.3\,\text{mm}\), the resolution was \(360\,\text{dpi}\), and the printhead width was \(1000\,\text{mm}\). The upper mould required 951 layers. The printing process was stable, and the printed upper mould had clear contours and no dragging defects. After printing, the mould was left to cure, cleaned, and coated with foundry coating.
6.6 Lower Mould by CNC Milling
The lower mould had no undercuts and could be machined by CNC milling. I selected three tools: a \(D50\) end mill for face and contour milling, a \(D20\) end mill for roughing, and a \(B8\) ball nose cutter for finishing. I generated the tool paths in CAM software and verified them for gouges and collisions. The lower mould was machined on the digital patternless casting machine. The machining process included tool setting, roughing, semi-finishing, finishing, and sand chip cleaning. The lower mould was completed in about one day.
6.7 Mould Assembly
After machining and printing, I cleaned the upper and lower sand moulds, applied foundry coating, and assembled them. The hybrid additive–subtractive route produced the complete sand mould in about one week. In contrast, conventional pattern-based sand mould casting often requires about two weeks. This demonstrated that additive and subtractive manufacturing can shorten the mould production cycle and reduce trial cost for single-piece and small-batch machine tool castings.
7. Orthogonal Optimization of Pouring Parameters
After selecting the gating system and optimizing the mould design, I further optimized the pouring parameters to reduce shrinkage porosity, residual stress, and deformation. I studied three factors: pouring temperature \(A\), pouring time \(B\), and sand mould preheating temperature \(C\). Each factor had five levels.
| Level | A: Pouring Temperature (\(^\circ\text{C}\)) | B: Pouring Time (s) | C: Mould Preheating Temperature (\(^\circ\text{C}\)) |
|---|---|---|---|
| 1 | 1360 | 20 | 430 |
| 2 | 1380 | 22 | 450 |
| 3 | 1400 | 24 | 470 |
| 4 | 1420 | 26 | 490 |
| 5 | 1440 | 28 | 510 |
I used an \(L_{25}(5^3)\) orthogonal array. The response variables were shrinkage porosity volume, residual stress, and deformation. Smaller values are better for all three responses. The simulation results are listed below.
| Run | A (\(^\circ\text{C}\)) | B (s) | C (\(^\circ\text{C}\)) | Porosity (\(\text{cm}^3\)) | Residual Stress (MPa) | Deformation (mm) |
|---|---|---|---|---|---|---|
| 1 | 1360 | 20 | 430 | 1.89 | 1446.0 | 2.13 |
| 2 | 1360 | 22 | 450 | 1.81 | 1320.6 | 2.15 |
| 3 | 1360 | 24 | 470 | 1.71 | 1379.8 | 2.22 |
| 4 | 1360 | 26 | 490 | 1.77 | 1318.7 | 2.31 |
| 5 | 1360 | 28 | 510 | 1.74 | 1272.4 | 2.30 |
| 6 | 1380 | 20 | 450 | 1.58 | 1396.8 | 2.13 |
| 7 | 1380 | 22 | 470 | 1.51 | 1369.4 | 2.18 |
| 8 | 1380 | 24 | 490 | 1.70 | 1340.4 | 2.23 |
| 9 | 1380 | 26 | 510 | 1.35 | 1264.1 | 2.33 |
| 10 | 1380 | 28 | 430 | 1.69 | 1374.5 | 2.05 |
| 11 | 1400 | 20 | 470 | 1.17 | 1336.1 | 2.24 |
| 12 | 1400 | 22 | 490 | 1.31 | 1327.8 | 2.26 |
| 13 | 1400 | 24 | 510 | 1.28 | 1236.5 | 2.33 |
| 14 | 1400 | 26 | 430 | 1.22 | 1330.4 | 2.16 |
| 15 | 1400 | 28 | 450 | 1.36 | 1398.5 | 2.17 |
| 16 | 1420 | 20 | 490 | 1.35 | 1278.2 | 2.27 |
| 17 | 1420 | 22 | 510 | 1.16 | 1206.8 | 2.33 |
| 18 | 1420 | 24 | 430 | 1.20 | 1295.2 | 2.08 |
| 19 | 1420 | 26 | 450 | 1.13 | 1369.3 | 2.19 |
| 20 | 1420 | 28 | 470 | 1.19 | 1316.2 | 2.24 |
| 21 | 1440 | 20 | 510 | 1.01 | 1173.7 | 2.32 |
| 22 | 1440 | 22 | 430 | 1.02 | 1426.4 | 2.09 |
| 23 | 1440 | 24 | 450 | 1.02 | 1373.9 | 2.16 |
| 24 | 1440 | 26 | 470 | 0.99 | 1293.4 | 2.26 |
| 25 | 1440 | 28 | 490 | 1.02 | 1289.9 | 2.25 |
7.1 Range Analysis
For each factor and each response, I calculated the average value at each level. The range \(R\) is the difference between the maximum and minimum average values. A larger range means a stronger influence. The results are summarized below.
| Response | Factor | Best Level | Range \(R\) | Influence Order |
|---|---|---|---|---|
| Porosity | A: Pouring temperature | A5 | 0.772 | A > C > B |
| Porosity | B: Pouring time | B4 | 0.108 | |
| Porosity | C: Mould preheating | C5 | 0.122 | |
| Residual stress | A: Pouring temperature | A4 | 55.9 | C > A > B |
| Residual stress | B: Pouring time | B4 | 15.12 | |
| Residual stress | C: Mould preheating | C5 | 143.8 | |
| Deformation | A: Pouring temperature | A2 | 0.016 | C > B > A |
| Deformation | B: Pouring time | B5 | 0.048 | |
| Deformation | C: Mould preheating | C1 | 0.220 |
For porosity alone, the best combination was \(A5B4C5\), namely \(1440^\circ\text{C}\), \(26\,\text{s}\), and \(510^\circ\text{C}\). For residual stress alone, the best combination was \(A4B4C5\), namely \(1420^\circ\text{C}\), \(26\,\text{s}\), and \(510^\circ\text{C}\). For deformation alone, the best combination was \(A2B5C1\), namely \(1380^\circ\text{C}\), \(28\,\text{s}\), and \(430^\circ\text{C}\). Because the three responses conflict, I used matrix analysis to obtain a balanced optimum.
7.2 Matrix Analysis
I constructed an index layer matrix \(M\), a factor layer matrix \(T\), and a level layer matrix \(E\). The weight matrix for each index is
$$\omega_i = M_i T_i E_i$$
For a smaller-is-better response, the index layer uses \(k_{ij} = 1/K_{ji}\). After normalizing and combining the three responses, I obtained the overall weight matrix \(\omega\). The largest weight for each factor was selected as the optimal level.
| Factor | Level 1 | Level 2 | Level 3 | Level 4 | Level 5 | Best Level |
|---|---|---|---|---|---|---|
| A: Pouring temperature | 0.0582 | 0.0635 | 0.0764 | 0.0768 | 0.0872 | A5 |
| B: Pouring time | 0.0230 | 0.0232 | 0.0231 | 0.0234 | 0.0230 | B4 |
| C: Mould preheating | 0.1052 | 0.1039 | 0.1038 | 0.1032 | 0.1057 | C5 |
The matrix analysis gave the optimal combination \(A5B4C5\): pouring temperature \(1440^\circ\text{C}\), pouring time \(26\,\text{s}\), and sand mould preheating temperature \(510^\circ\text{C}\). This combination provided the best overall balance among shrinkage porosity, residual stress, and deformation.
7.3 Verification of the Optimal Parameters
I ran a final simulation with the optimal parameters. The results are compared with the pre-optimization values below.
| Item | Before Parameter Optimization | After Parameter Optimization |
|---|---|---|
| Shrinkage porosity volume (\(\text{cm}^3\)) | 1.42 | 1.00 |
| Maximum residual stress (MPa) | 1351.1 | 1178.7 |
| Maximum deformation (mm) | 2.32 | 2.22 |
The optimized parameters reduced shrinkage porosity, residual stress, and deformation. The final sand mould casting process therefore combined a parting gating system, chills, insulating risers, vents, and optimized pouring parameters.
8. Discussion
The results show that sand mould casting of a large machine tool slide seat can be significantly improved by combining numerical simulation with advanced mould manufacturing. The parting gating system was better than the top and bottom systems because it provided stable filling and a more balanced thermal field. The top gating system caused slight splashing, while the bottom gating system left the bottom region superheated and delayed solidification. These effects are common in sand mould casting of heavy machine tool parts.
The addition of chills and insulating risers changed the solidification sequence. Chills increased the cooling rate in thick sections, while risers provided liquid feeding to the last solidifying regions. Vents reduced gas pressure and helped prevent gas-related defects. The shrinkage porosity volume dropped from \(132.58\,\text{cm}^3\) to \(1.42\,\text{cm}^3\), which is a major improvement for sand mould casting.
The hybrid additive–subtractive mould manufacturing route also proved effective. The upper mould had undercuts and complex details, so 3D sand printing was suitable. The lower mould had no undercuts and could be machined efficiently by CNC milling. This hybrid method reduced the mould production cycle to about one week and avoided the need for a conventional pattern. It is especially suitable for single-piece and small-batch sand mould casting of machine tool components.
The orthogonal experiment showed that pouring temperature had the strongest effect on shrinkage porosity, sand mould preheating temperature had the strongest effect on residual stress and deformation, and pouring time had a relatively smaller effect. The matrix analysis provided a balanced optimum: \(1440^\circ\text{C}\), \(26\,\text{s}\), and \(510^\circ\text{C}\). This combination further reduced the defect levels.
9. Conclusions
I drew the following conclusions from this study:
1. For the machine tool slide seat, HT250 gray cast iron is a suitable material for sand mould casting because it offers good fluidity, low shrinkage, and adequate strength. The main casting parameters were a pouring temperature of \(1370\text{–}1440^\circ\text{C}\), a pouring time of \(24\,\text{s}\), and a sand mould preheating temperature of \(430\text{–}510^\circ\text{C}\).
2. Among the top, parting, and bottom gating systems, the parting gating system produced the most stable filling and the smallest shrinkage porosity volume. It was selected as the best design for sand mould casting.
3. Adding chills, insulating risers, and vents greatly reduced shrinkage porosity. The predicted porosity volume decreased from \(132.58\,\text{cm}^3\) to \(1.42\,\text{cm}^3\). The optimized solidification sequence promoted feeding and reduced hot spots.
4. The hybrid additive–subtractive method successfully manufactured the upper and lower sand moulds. The upper mould was 3D printed, and the lower mould was CNC milled. This route shortened the mould production cycle and reduced cost and labor intensity for sand mould casting.
5. The orthogonal experiment and matrix analysis gave the optimal pouring parameters: pouring temperature \(1440^\circ\text{C}\), pouring time \(26\,\text{s}\), and sand mould preheating temperature \(510^\circ\text{C}\). Under these conditions, the shrinkage porosity volume was reduced to \(1.00\,\text{cm}^3\), the maximum residual stress to \(1178.7\,\text{MPa}\), and the maximum deformation to \(2.22\,\text{mm}\).
10. Future Work
Although the numerical simulation and mould manufacturing results are promising, several aspects can be improved. First, I treated the interfacial heat transfer coefficients as constant values. In real sand mould casting, these coefficients vary with temperature and contact conditions. Future work should use temperature-dependent interfacial parameters. Second, the predicted residual stress was still relatively high compared with some published gray iron castings. Further work should investigate mould constraint, shakeout time, and cooling rate effects to reduce residual stress. Third, because of time and experimental limitations, I did not perform an actual pour and compare the final casting with the simulation. Future work should include experimental validation by pouring the slide seat and measuring shrinkage porosity, residual stress, and deformation. These improvements will make the sand mould casting process more reliable for industrial production.