Controlling Porosity Defects in ZG1Cr10MoVNbN Steel Castings

I have been directly involved in the development and industrial production of ZG1Cr10MoVNbN high-alloy heat-resistant steel castings for supercritical and ultra-supercritical steam turbine components. This material is a martensitic heat-resistant cast steel strengthened by a multi-element Cr-Mo-Ni-Nb-V-N composite system. It offers high strength, toughness, creep resistance, and good resistance to high-temperature oxidation and corrosion. It is widely used for high-pressure cylinder bodies, high-pressure main steam valves, regulating valves, and high-temperature diaphragms. However, its high alloy content and strict requirements for alloying element control, mechanical properties, and nitrogen content make production difficult. In particular, the presence of nitrogen makes the material highly susceptible to gas porosity. Through systematic research on the role of each alloying element, I established internal chemical composition limits, a melting process, and a casting process that form a mature production technology. The central problem I address here is the formation and control of casting defects, especially porosity, in ZG1Cr10MoVNbN supercritical martensitic stainless steel castings.

Porosity is one of the most damaging casting defects in this material because it significantly reduces high-temperature fatigue performance and corrosion resistance. The presence of casting defects such as gas holes and shrinkage porosity can lead to premature failure under supercritical operating conditions. Therefore, my work has focused on understanding the root causes of these casting defects and on implementing effective countermeasures in both the foundry and the melting shop. In the following sections, I present the causes of porosity, the casting process improvements, the melting and refining strategy, the internal control composition, and the actual production verification data.

1. Casting Process Aspects

1.1 Causes of Defect Formation

For a main regulating valve housing used in large thermal power generation projects, I selected a resin-bonded sand molding process based on the product size, wall thickness, and structure. I analyzed the reasons for casting defects such as gas porosity and shrinkage porosity in the castings. The main causes were as follows. First, the resin addition in the molding sand was too high, which greatly increased the gas evolution from the sand cores. Second, the drying of the cores was insufficient, so a large amount of gas was already present in the mold cavity before the alloy liquid entered. Third, the gating system design was unreasonable, causing gas in the mold cavity to enter the alloy liquid after pouring, and making it difficult for gas in the alloy liquid to escape. Fourth, the internal cylinder valve body of this model is particularly thick and large, so the solidification time was too long. As the temperature decreased during solidification, the gas saturation in the solution dropped sharply. After solidification was completed, a large amount of gas precipitated, producing numerous gas porosity casting defects.

From a physical chemistry perspective, the solubility of gases in liquid steel decreases with decreasing temperature. The precipitation of gas during solidification can be described by Sieverts’ law for diatomic gases:

$$ [\%H] = K_H \sqrt{P_{H_2}} $$

$$ [\%N] = K_N \sqrt{P_{N_2}} $$

where \( [\%H] \) and \( [\%N] \) are the dissolved gas concentrations, \( K_H \) and \( K_N \) are temperature-dependent equilibrium constants, and \( P_{H_2} \) and \( P_{N_2} \) are the partial pressures of the gases. As the temperature falls, \( K_H \) and \( K_N \) decrease, so the equilibrium gas concentration decreases. If the actual gas content exceeds the equilibrium value, gas bubbles form. These bubbles become trapped during solidification and appear as casting defects. For a thick section, the local solidification time is long, which allows more gas to diffuse and accumulate, increasing the severity of porosity casting defects.

Moreover, the resin binder decomposes when it contacts the molten metal, generating gases such as \( H_2 \), \( CO \), \( CO_2 \), and hydrocarbons. The gas evolution volume can be approximated by:

$$ V_g = m_b \cdot G_b $$

where \( V_g \) is the gas volume, \( m_b \) is the mass of binder, and \( G_b \) is the specific gas evolution of the binder. Reducing the binder mass and ensuring complete core drying directly lower \( V_g \). This was one of the key measures I adopted.

1.2 Measures Taken

To address the causes of porosity casting defects in this material, I implemented the following measures:

  • I reasonably controlled the resin addition in the molding sand to reduce gas evolution from the sand.
  • I strengthened the drying of the sand cores to reduce the gas evolution from the molding sand.
  • I optimized the gating system design by using a stepped gate plus a slag-collecting ladle to reduce turbulent gas entrainment. At the same time, I placed multiple vent holes in the upper mold to facilitate the escape of gas from the alloy liquid.
  • I placed chromite sand and chills at critical positions to increase the solidification rate by about 30%, thereby suppressing gas precipitation.

These changes significantly reduced the formation of casting defects. The solidification rate increase can be understood through the relationship between solidification time and section modulus. For a given casting modulus \( M = V/A \), the solidification time \( t_s \) is approximately:

$$ t_s = k M^n $$

where \( k \) is a constant depending on the mold material and metal, and \( n \) is usually between 1.5 and 2. By using chromite sand and chills, the effective \( k \) is reduced, so \( t_s \) becomes shorter. A shorter solidification time limits gas diffusion and reduces the probability of porosity casting defects. In the actual production, the local solidification rate increased by about 30%, which was sufficient to suppress gas precipitation in the thick sections.

In addition to the above measures, I carefully controlled the pouring temperature. A lower pouring temperature reduces the gas solubility and the tendency for secondary oxidation and gas entrainment, but it must still satisfy the filling requirements. I determined the pouring temperature according to the casting structure, size, and wall thickness. This balance is critical for minimizing casting defects while ensuring complete mold filling.

2. Melting Process Aspects

ZG1Cr10MoVNbN supercritical martensitic stainless steel contains a certain amount of nitrogen and also contains elements such as V and Nb that are easily oxidized at high temperatures. Strictly controlling impurity and gas contents during melting is one of the prerequisites for obtaining high-quality castings. Generally, a medium-frequency induction furnace can also produce acceptable castings. However, when melting in a medium-frequency induction furnace, special attention must be paid to oxidation and gas absorption. I controlled the impurity and gas contents of raw materials, used a covering agent to isolate the air, applied inert gas protection around the furnace mouth, and shortened the melting time. These measures improve the quality of the molten metal.

Nevertheless, the strong electromagnetic stirring in a medium-frequency induction furnace produces a “hump” phenomenon. This exposes the steel liquid to the atmosphere for a long time, increasing the gas content and making it difficult to remove. During solidification, a large number of gas pores form, or many inclusions form at grain boundaries, severely degrading the alloy properties. Therefore, for the production of ZG1Cr10MoVNbN supercritical martensitic stainless steel, I adopted a process route of medium-frequency furnace primary melting plus AOD ladle refining. This greatly reduced the O and H gas contents in the steel liquid and produced high-quality castings with minimal casting defects.

2.1 Role of Elements and Internal Control Composition

I studied the role of each element in the steel and established the internal control composition. The roles are as follows:

  • C: Forms the strengthening phase and is essential for the martensitic matrix and various carbides. It directly affects strength and hardness. The content must be precisely controlled. If it is too low, strength is insufficient; if it is too high, toughness is impaired. I found that about 0.12% C gives a good combination of properties.
  • Cr: Provides corrosion and oxidation resistance. It forms a dense oxide film on the steel surface and is the main element for improving corrosion resistance. At a sufficient content, it helps refine the structure and keeps the steel stable in high-temperature steam environments.
  • Mo: Provides solid-solution strengthening and improves hot strength. By dissolving in the matrix, it significantly increases high-temperature strength and creep resistance.
  • V and Nb: Provide precipitation strengthening and grain refinement. They form fine, dispersed (Nb,V)(C,N) composite precipitates, which reduce the free N content.
  • N: Provides auxiliary precipitation strengthening and solid-solution strengthening. It forms more stable carbonitrides with V and Nb, enhancing precipitation strengthening. It also partially dissolves in the matrix for strengthening.

Based on this analysis, I established a reasonable internal control composition for ZG1Cr10MoVNbN supercritical martensitic stainless steel. The target composition is shown in Table 1.

Table 1. Internal control chemical composition of ZG1Cr10MoVNbN alloy (mass fraction, %)
C Mn Si S P Cr Mo Ni V Nb N
0.10–0.13 0.50–0.70 0.40–0.60 ≤ 0.005 ≤ 0.025 9.20–9.80 0.70–0.90 0.45–0.65 0.13–0.18 0.040–0.060 0.040–0.060

The internal control composition is tighter than the general specification. This is necessary because small variations in C, N, V, and Nb can strongly affect the precipitation kinetics and the tendency for casting defects. For example, if N is too high, the risk of gas porosity increases. If N is too low, the precipitation strengthening is insufficient. The narrow ranges in Table 1 reflect the need to balance mechanical properties and castability.

2.2 Medium-Frequency Furnace Primary Melting

For the medium-frequency furnace primary melting, I followed these steps:

  • Batching: According to the production plan, I batched each furnace based on the internal control composition. I prepared all raw materials required for medium-frequency furnace melting. Ferroalloys and return material of the same steel grade had to be clean, dry, and free of oil and grease.
  • Charging: I first added about 0.5% of the furnace charge as a covering agent or refining agent with deoxidation and desulfurization functions, such as calcium oxide or a mixture of calcium oxide and magnesium oxide. Then I added scrap steel, ferrochrome, nickel, ferromolybdenum, return material, and electrolytic manganese. The primary molten steel had to contain a certain amount of carbon. Other components were charged according to the middle to lower limits of the internal control requirements.

The tapping temperature of the medium-frequency furnace must be appropriate, and the tundish must be well preheated. During melting, I controlled the furnace power and kept stirring stable. If a “hump” appeared, I continuously added a covering agent for protection. The “hump” causes the covering slag on the melt surface to break. I tried to shorten the melting time as much as possible. Increasing the frequency can reduce the height of the “hump.” Because the melting amount of the induction furnace is reduced, the crucible capacity must be correspondingly reduced. It is also possible to add a suitable crucible sleeve section on the induction coil to use the gravity of the liquid above the induction coil to eliminate the influence of the “hump.” These operational details are important because they directly influence gas absorption and the subsequent formation of casting defects.

The electromagnetic stirring in the medium-frequency furnace can be described by the magnetic Reynolds number and the resulting flow pattern, but the practical consequence is the “hump.” The gas absorption rate can be expressed as:

$$ \frac{d[\%O]}{dt} = k_O A ( [\%O]_s – [\%O] ) $$

where \( k_O \) is the mass transfer coefficient, \( A \) is the exposed surface area, \( [\%O]_s \) is the surface oxygen concentration, and \( [\%O] \) is the bulk oxygen concentration. The “hump” increases \( A \), so the oxygen absorption rate increases. Covering agents reduce \( A \) and lower the oxygen pickup. This is why I paid close attention to covering and stirring stability.

2.3 AOD Ladle Refining

AOD ladle refining has great advantages for stainless steel. When oxygen is blown into the steel liquid, the decarburization reaction is:

$$ [C] + [O] = CO(g) $$

By blowing argon, the CO partial pressure can be reduced, which promotes the reaction to completion. At the same time, the gas is blown into the depths of the molten pool at high speed, allowing the steel liquid and slag to mix fully. This increases the reaction rate in the molten pool, so the carbon content can be rapidly reduced to below 0.01%. The equilibrium constant for decarburization can be written as:

$$ K = \frac{P_{CO}}{a_C a_O} $$

where \( a_C \) and \( a_O \) are the activities of carbon and oxygen, and \( P_{CO} \) is the CO partial pressure. By diluting CO with argon, \( P_{CO} \) is lowered, and the equilibrium shifts toward CO formation, thereby removing carbon. At the same time, the argon bubbles act as countless small vacuum chambers. Oxygen, hydrogen, and CO diffuse into the argon bubbles. As the bubbles rise, they stir the steel liquid, and inclusions float up into the slag. The cleanliness of the steel liquid is therefore improved. This is a key step for reducing casting defects, because cleaner steel has less gas and fewer inclusions that can form porosity.

During AOD reduction, under strong argon stirring, the steel and slag mix well, and the desulfurization effect is very good. The sulfur content can be reduced to below \( 10 \times 10^{-6} \). Another major advantage of the AOD refining process is the adjustment of nitrogen in the steel. Nitrogen gas can be blown directly into the furnace to replace traditional nitrogen-containing ferrochrome. This is convenient and low in cost. The nitrogen content can be controlled by the partial pressure of nitrogen according to:

$$ [\%N] = K_N \sqrt{P_{N_2}} $$

I used this relationship to adjust the nitrogen level precisely. Because nitrogen is both a strengthening element and a cause of gas porosity, this control is critical. If the nitrogen content is too high, gas porosity casting defects become more likely. If it is too low, the required high-temperature strength may not be achieved.

Before the molten metal enters the AOD, I ensured that the AOD furnace had been baked for more than 3 hours. I ensured that the furnace temperature was above 800 °C when the molten metal entered. I added about 5% of the steel liquid mass as lime at the furnace bottom, and the lime was baked together with the furnace. For a newly lined furnace (magnesia-calcium brick), the baking time had to be more than 24 hours. After charging, I used an Ar/O₂ ratio of 1/4 for oxygen blowing and decarburization. The first stage mainly involved heating, slag melting, and stirring. Then I gradually adjusted the Ar/O₂ ratio until the carbon was reduced to below 0.08%. I then stirred with pure argon and entered the reduction period. During the reduction period, I calculated the required aluminum and lime amounts based on the oxygen consumption in the oxidation period and the steel liquid mass. The argon stirring time was determined by the steel liquid mass. I took samples for chemical analysis. According to the analysis results, I made fine adjustments to the composition and took a full analysis sample. Only after the composition met the internal control requirements, especially the N content, did I tap the steel. The pouring temperature was determined according to the casting structure, size, and wall thickness.

After AOD refining, the steel liquid has been stirred by argon. The numerous argon bubbles act like countless vacuum chambers. Oxygen, hydrogen, and CO diffuse into the argon bubbles. The rising bubbles stir the steel liquid, and inclusions float into the slag. The cleanliness of the steel liquid is improved. Under the premise of ensuring casting filling, I appropriately lowered the pouring temperature. This reduced secondary oxidation and gas entrainment and helped reduce casting defects such as gas porosity. The relationship between pouring temperature and gas solubility is:

$$ \log [\%H] = -\frac{A}{T} + B $$

where \( T \) is the absolute temperature, and \( A \) and \( B \) are constants. Lowering the temperature reduces hydrogen solubility. However, if the temperature is too low, misruns and cold shuts may occur. I therefore optimized the pouring temperature to balance filling and gas control.

3. Heat Treatment and Actual Production Verification

The preliminary heat treatment for this material is high-temperature annealing. After high-temperature annealing, the furnace is cooled to below 250 °C before being taken out. The final heat treatment process is normalizing at \( 1090 \pm 10 \) °C plus tempering at \( 710 \pm 10 \) °C. This heat treatment provides the desired martensitic structure and precipitation strengthening. It also helps to relieve stresses and improve toughness.

To verify the practical application effect of the proposed casting process and melting process, I carried out multiple industrial production heats of ZG1Cr10MoVNbN alloy according to the process route described above. All production heats used the medium-frequency furnace primary melting plus AOD refining process and followed the internal control chemical composition and heat treatment schedule. From the continuous production heats, I selected four representative heats for analysis. The actual chemical compositions are shown in Table 2.

Table 2. Actual chemical composition of production heats (mass fraction, %)
Heat No. Material C Mn Si P S Cr Mo Ni V Nb N
Y39058 ZG1Cr10MoVNbN 0.118 0.65 0.46 0.018 0.001 9.58 0.82 0.52 0.17 0.045 0.041
Y39134 ZG1Cr10MoVNbN 0.116 0.63 0.47 0.020 0.001 9.67 0.85 0.51 0.16 0.047 0.043
Y39386 ZG1Cr10MoVNbN 0.124 0.67 0.44 0.018 0.001 9.53 0.83 0.55 0.17 0.045 0.042
Y39593 ZG1Cr10MoVNbN 0.121 0.65 0.46 0.019 0.001 9.74 0.86 0.52 0.15 0.048 0.042

All four heats met the internal control composition requirements. The carbon content was between 0.116% and 0.124%, the chromium content was between 9.53% and 9.74%, and the nitrogen content was between 0.041% and 0.043%. These values are within the narrow ranges specified in Table 1. The low sulfur and phosphorus contents confirm the effectiveness of the AOD refining and raw material control. The controlled nitrogen content is particularly important because it directly affects both precipitation strengthening and the risk of gas porosity casting defects.

The four castings were heat treated by normalizing at \( 1090 \pm 10 \) °C and tempering at \( 710 \pm 10 \) °C. High-temperature creep rupture tests were carried out at 630 °C, 650 °C, and 660 °C according to the standard. The results are shown in Table 3.

Table 3. Actual high-temperature creep rupture properties
Heat No. Material Temperature / °C Stress / N·mm⁻² Standard requirement / h Actual time / h Remarks
Y39058 ZG1Cr10MoVNbN 630 147 ≥50 55 Manually fractured
Y39058 ZG1Cr10MoVNbN 650 123 ≥80 90 Manually fractured
Y39058 ZG1Cr10MoVNbN 660 98 ≥200 230 Manually fractured
Y39134 ZG1Cr10MoVNbN 630 147 ≥50 53 Manually fractured
Y39134 ZG1Cr10MoVNbN 650 123 ≥80 88 Manually fractured
Y39134 ZG1Cr10MoVNbN 660 98 ≥200 235 Manually fractured
Y39386 ZG1Cr10MoVNbN 630 147 ≥50 58 Manually fractured
Y39386 ZG1Cr10MoVNbN 650 123 ≥80 91 Manually fractured
Y39386 ZG1Cr10MoVNbN 660 98 ≥200 235 Manually fractured
Y39593 ZG1Cr10MoVNbN 630 147 ≥50 60 Manually fractured
Y39593 ZG1Cr10MoVNbN 650 123 ≥80 90 Manually fractured
Y39593 ZG1Cr10MoVNbN 660 98 ≥200 240 Manually fractured

By strictly controlling the quality of raw materials, optimizing the internal control chemical composition, and applying the AOD refining process, the cleanliness of the steel liquid was improved. As shown in Table 3, the following results were obtained. At 630 °C and 147 MPa, the high-temperature creep rupture life of the four heats reached 53–60 h, which is higher than the standard requirement of 50 h. At 650 °C and 123 MPa, the life reached 88–91 h, which is higher than the standard requirement of 80 h. At 660 °C and 98 MPa, the life reached 230–240 h, which is higher than the standard requirement of 200 h. These results indicate that the process can stably produce castings that meet the required high-temperature creep rupture properties. In other words, the reduction of casting defects and the improvement of steel cleanliness directly contributed to the excellent high-temperature performance.

The actual production products were inspected. Radiographic testing (RT) and penetrant testing (PT) were performed. No gas porosity, shrinkage porosity, or other casting defects were found. The quality was significantly improved. This confirms that the combination of optimized casting process and medium-frequency furnace primary melting plus AOD refining is effective for controlling casting defects in ZG1Cr10MoVNbN supercritical martensitic stainless steel castings.

4. Discussion

The control of casting defects in ZG1Cr10MoVNbN requires an integrated approach. I have found that casting defects such as gas porosity originate from multiple sources: gas evolution from the sand mold and cores, gas entrainment during pouring, gas precipitation during solidification, and residual gas and inclusions in the molten steel. Each source must be addressed. In the casting process, the key measures are reducing resin addition, drying cores thoroughly, optimizing gating to reduce turbulence, adding vents, and using chills and chromite sand to increase the solidification rate. In the melting process, the key measures are strict raw material control, internal composition control, medium-frequency furnace primary melting with covering and inert gas protection, and AOD refining to reduce O, H, and S while precisely adjusting N.

The thermodynamics and kinetics of gas porosity can be summarized by the following relationships. The gas solubility decreases with temperature, so gas precipitation occurs when the actual gas content exceeds the equilibrium value at the solidification front. The supersaturation ratio can be defined as:

$$ S = \frac{C_{\text{actual}}}{C_{\text{eq}}} $$

When \( S > 1 \), gas bubbles tend to form. The critical bubble radius \( r_c \) for nucleation is:

$$ r_c = \frac{2\sigma}{\Delta P} $$

where \( \sigma \) is the surface tension and \( \Delta P \) is the pressure difference. If the supersaturation is high, \( \Delta P \) is large, and \( r_c \) is small, so nucleation is easier. This explains why thick sections with long solidification times are more susceptible to gas porosity casting defects. By increasing the solidification rate, I reduced the time available for gas diffusion and bubble growth. By reducing the gas content in the steel, I lowered \( S \) and \( \Delta P \), making nucleation less likely. By reducing turbulence and gas entrainment, I reduced the initial gas content. These mechanisms are all consistent with the observed reduction in casting defects.

For AOD refining, the decarburization and degassing reactions are central. The carbon-oxygen reaction is:

$$ [C] + [O] = CO(g) $$

The equilibrium constant is:

$$ K = \frac{P_{CO}}{a_C a_O} $$

By blowing argon, the CO partial pressure is reduced, and the equilibrium shifts to the right. The oxygen content is also reduced. The hydrogen and nitrogen contents are controlled by Sieverts’ law:

$$ [\%H] = K_H \sqrt{P_{H_2}} $$

$$ [\%N] = K_N \sqrt{P_{N_2}} $$

By using argon and nitrogen gas mixtures, I controlled the nitrogen partial pressure and thus the nitrogen content. This is a precise way to achieve the target nitrogen range without adding nitrogen-bearing ferroalloys that can introduce impurities. The AOD process also provides strong stirring, which increases the reaction rates and helps remove inclusions. The cleanliness of the steel is therefore improved, and the casting defects are reduced.

Table 4 summarizes the main process measures and their effects on casting defects.

Table 4. Summary of measures and effects on casting defects
Process Area Measure Mechanism Effect on Casting Defects
Molding sand Reduce resin addition Lower gas evolution Fewer gas porosity defects
Core drying Strengthen drying Remove moisture and volatiles Lower gas content in mold cavity
Gating system Stepped gate + slag-collecting ladle Reduce turbulence and gas entrainment Fewer gas and inclusion defects
Venting Multiple vent holes in upper mold Facilitate gas escape Lower gas pressure in mold cavity
Solidification Chromite sand and chills Increase solidification rate by 30% Suppress gas precipitation
Melting Medium-frequency furnace with covering and inert gas Reduce oxidation and gas absorption Lower gas content in steel
Refining AOD with Ar/O₂ and Ar stirring Reduce CO partial pressure, remove O, H, S Improve steel cleanliness, reduce porosity defects
Composition control Internal control range for C, Cr, Mo, V, Nb, N Balance strengthening and gas control Minimize casting defects and meet properties
Pouring Optimized pouring temperature Lower gas solubility and secondary oxidation Reduce gas porosity and entrainment defects
Heat treatment Normalizing + tempering Optimize microstructure and precipitates Improve performance, no direct defect formation

The actual production data in Tables 2 and 3 confirm the effectiveness of the integrated approach. The chemical compositions are within the internal control limits, and the high-temperature creep rupture lives exceed the standard requirements at all three test conditions. The RT and PT inspections found no gas porosity or shrinkage porosity. Therefore, the process route is stable and suitable for industrial production.

5. Conclusion

I addressed the problem of casting defects, especially gas porosity, in ZG1Cr10MoVNbN supercritical martensitic stainless steel castings. I analyzed the effects of sand gas evolution, gating system design, solidification process, and steel cleanliness on porosity formation. I proposed corresponding process control measures. The main conclusions are as follows.

  1. The causes of porosity casting defects include high resin addition, insufficient core drying, unreasonable gating, long solidification time in thick sections, and high gas content in the steel liquid. These factors increase gas evolution, gas entrainment, and gas precipitation.
  2. By optimizing the casting process and adopting medium-frequency furnace primary melting plus AOD refining, I effectively reduced the gas and non-metallic inclusion contents in the steel liquid. The steel cleanliness was improved, and the casting forming quality was improved. The actual castings showed no gas porosity or shrinkage porosity in RT and PT inspections.
  3. The industrial production results showed that four heats met the internal control composition requirements. The high-temperature creep rupture lives at 630 °C, 650 °C, and 660 °C all met or exceeded the standard requirements. This indicates that the process can stably produce ZG1Cr10MoVNbN martensitic stainless steel castings that meet the requirements of supercritical units. The process has good engineering application value.

The key to controlling casting defects in this material is to combine careful foundry practice with precise melting and refining. The internal control composition in Table 1, the AOD refining parameters, the gating and venting design, and the use of chills and chromite sand all contribute to the final result. The reduction of casting defects is not achieved by a single measure but by the integration of multiple measures that address gas sources, gas entrainment, gas precipitation, and steel cleanliness simultaneously. I believe that the approach described here can be applied to other high-alloy heat-resistant steel castings with similar challenges.

In future production, I will continue to monitor the nitrogen content and the gas content in the steel liquid, because these are the most critical variables for porosity casting defects. I will also further optimize the pouring temperature and the solidification rate for different wall thicknesses. The goal is to achieve consistent zero-defect production and to meet the increasingly stringent requirements of supercritical and ultra-supercritical power generation equipment.