Optimization of Investment Casting Process for Fixed Disk Using Numerical Simulation and Orthogonal Experiment

In modern automotive applications, the stability and reliability of components are critical due to complex operating conditions. The fixed disk, which supports the air conditioning compressor, is subject to variable environmental stresses, necessitating advanced manufacturing techniques. Precision casting, particularly investment casting, is widely employed for producing intricate parts with high dimensional accuracy. This study focuses on designing and optimizing the investment casting process for a fixed disk using ProCAST software, integrating numerical simulation with orthogonal experiments to minimize defects such as shrinkage porosity and cavities. The methodology emphasizes the synergy between precision casting and investment casting to enhance product quality.

The fixed disk is fabricated from JDMB2K4140 alloy steel, equivalent to AISI 4140 or ISO 42CrMo4 steel, with a chemical composition detailed in Table 1. This material is selected for its excellent mechanical properties, including high strength and toughness, which are essential for automotive components. The casting features a complex geometry with uniform wall thickness averaging 7 mm, and includes a 15 mm diameter through-hole. Its maximum dimensions are 126 mm × 75 mm × 72 mm. Defects like slag inclusions and cracks must be avoided to ensure structural integrity. A three-dimensional model, developed using UGNX10.0, illustrates the part’s intricate design, highlighting the need for precision casting techniques to achieve high-quality outcomes.

Table 1: Chemical Composition of 42CrMo4 Alloy Steel (wt%)
C Si Mn Cr Mo P S Ni Cu
0.38–0.45 0.17–0.37 0.50–0.80 0.90–1.20 0.15–0.25 ≤0.035 ≤0.035 ≤0.30 ≤0.30

The investment casting process begins with the design of the gating system, which is crucial for controlling metal flow and solidification. A sprue-runner-ingate configuration is adopted to promote sequential solidification and reduce shrinkage defects. This approach aligns with the principles of precision casting, ensuring smooth filling and adequate feeding. The three-dimensional finite element model of the gating system, as shown in the figure below, is meshed with a element size of 5 mm, resulting in 56,352 elements and 435,310 nodes. This model serves as the basis for simulation in ProCAST, where parameters such as heat transfer coefficients and boundary conditions are defined to replicate real-world investment casting conditions.

Key simulation parameters include an ambient temperature of 800°C, a shell thickness of 6 mm (composed of quartz sand and silica sol), and a material designation of 42CrMo4 steel. The pouring temperature is set to 1580°C, based on the alloy’s liquidus temperature of 1494°C and solidus temperature of 1425°C. Gravity is applied at 9.8 m/s² in the negative x-direction, while heat transfer coefficients are set to 500 W/(m²·K) for the shell and 1000 W/(m²·K) for air interactions. These settings ensure accurate modeling of the investment casting process, critical for precision casting applications. The initial pouring speed is determined using the empirical formula by Kalkin:

$$v = \frac{0.22 \sqrt{h}}{\delta \cdot \ln \frac{T}{380}}$$

where \( v \) is the pouring speed in cm/s, \( h \) is the casting height in cm, \( \delta \) is the wall thickness in cm, and \( T \) is the pouring temperature in °C. For the fixed disk, with \( h = 7.2 \, \text{cm} \), \( \delta = 0.7 \, \text{cm} \), and \( T = 1580°C \), the calculated speed is approximately 266 mm/s. To account for practical variations, an initial speed of 300 mm/s is used in simulations. The filling process is analyzed over 4 seconds, revealing a steady flow without turbulent impacts, which is essential for avoiding defects in investment casting. By 3.826 seconds, the mold is nearly fully filled, demonstrating the efficiency of the gating design in precision casting.

Solidification analysis indicates that the casting begins to solidify at the outer regions within 4 seconds, with complete solidification of the part achieved by 48 seconds and the entire system by 468 seconds. This sequential solidification pattern, from the casting inward to the sprue, favors the reduction of internal defects. However, shrinkage porosity and cavities are predicted in the curved sections and main sprue, as shown in the simulation results. These defects, common in investment casting, can compromise mechanical performance, underscoring the need for process optimization in precision casting. The initial process parameters, while functional, highlight areas for improvement through systematic experimentation.

To optimize the investment casting process, an orthogonal experiment is designed with three key factors: pouring temperature, pouring speed, and shell preheat temperature. Each factor is tested at three levels, as outlined in Table 2. The selection of levels is based on industry standards for precision casting; for instance, pouring temperatures are set 50–100°C above the liquidus temperature, shell preheat temperatures are elevated to 900–1100°C for thin-walled parts, and pouring speeds range from 200 to 400 mm/s to balance filling quality and efficiency.

Table 2: Factors and Levels for Orthogonal Experiment
Level Factor A: Pouring Temperature (°C) Factor B: Pouring Speed (mm/s) Factor C: Shell Preheat Temperature (°C)
1 1550 200 900
2 1560 300 1000
3 1580 400 1100

The L9(3^3) orthogonal array is employed, resulting in nine experimental schemes. Each scheme is simulated in ProCAST, and the results, including filling time and shrinkage porosity percentage, are recorded in Table 3. Shrinkage porosity is calculated as the sum of pore volume fractions exceeding 1.0%, with lower values indicating better quality in investment casting. For example, Scheme L5 shows the minimum shrinkage porosity of 1.7984%, while L2 exhibits the maximum at 1.9368%, demonstrating the impact of parameter variations on precision casting outcomes.

Table 3: Orthogonal Experiment Schemes and Results
Experiment Factor A Factor B Factor C Filling Time (s) Shrinkage Porosity (%)
L1 1 1 1 3.9216 1.8529
L2 1 2 2 3.7005 1.9368
L3 1 3 3 3.3782 1.8499
L4 2 1 2 3.1731 1.8775
L5 2 2 3 3.7413 1.7984
L6 2 3 1 3.6028 1.8182
L7 3 1 3 3.5219 1.8972
L8 3 2 2 3.3782 1.9170
L9 3 3 1 3.0732 1.8877

Range analysis of the orthogonal experiment results identifies the optimal parameter combination as A2B2C3, corresponding to a pouring temperature of 1560°C, pouring speed of 300 mm/s, and shell preheat temperature of 1100°C. This combination yields a shrinkage porosity of 1.80%, a filling time of 3.74 s, and a solidification time of 368.67 s, as summarized in Table 4. The improved process demonstrates enhanced filling and solidification characteristics, with reduced defects in critical areas like the curved sections. This optimization underscores the effectiveness of integrating numerical simulation with orthogonal experiments in investment casting for precision casting applications.

Table 4: Optimal Process Parameters for Investment Casting
Parameter Shell Thickness (mm) Shell Preheat Temperature (°C) Pouring Temperature (°C) Pouring Speed (mm/s) Filling Time (s) Solidification Time (s) Shrinkage Porosity (%)
Value 6 1100 1560 300 3.74 368.67 1.80

The superiority of the optimized investment casting process is evident in the simulation results. Filling occurs smoothly within 3.74 seconds, with metal flow remaining laminar and free of turbulence. Solidification progresses sequentially from the casting exterior to the sprue, minimizing thermal gradients and associated defects. Shrinkage porosity is concentrated in non-critical regions, with a significant reduction compared to the initial process. These outcomes validate the role of precision casting parameters in achieving high-quality components. The mathematical foundation of the optimization, including the Kalkin formula and statistical analysis, provides a reproducible framework for similar investment casting projects.

In conclusion, this study successfully optimizes the investment casting process for a fixed disk using ProCAST software and orthogonal experiments. The optimal parameters—shell thickness of 6 mm, shell preheat temperature of 1100°C, pouring temperature of 1560°C, and pouring speed of 300 mm/s—result in minimal defects and efficient production. The methodology highlights the importance of parameter prioritization in precision casting, where factors like pouring temperature and shell preheat temperature significantly influence outcomes. By leveraging numerical simulation, this approach reduces trial-and-error in investment casting, offering a reliable strategy for enhancing automotive component manufacturing. Future work could explore additional factors, such as cooling rates and alloy modifications, to further advance precision casting techniques.

Scroll to Top