Optimization of Medium Temperature Zinc-Calcium-Manganese Phosphating for Grey Iron Castings

In industrial applications, particularly for engine components, grey iron castings are widely utilized due to their favorable castability, damping capacity, and cost-efficiency. However, the presence of graphite in grey iron castings poses significant challenges for surface treatments, as it can hinder the adhesion and uniformity of protective coatings. Phosphating, a common pretreatment before painting, is employed to enhance corrosion resistance by forming a crystalline phosphate layer. Traditional phosphating processes for steel, such as high-temperature manganese-based and medium-temperature zinc-based systems, are not always optimal for grey iron castings. This study focuses on optimizing a medium-temperature zinc-calcium-manganese phosphating process specifically tailored for HT250 grey iron castings, aiming to achieve a fine and dense phosphate film with superior corrosion resistance. The optimization involves orthogonal experiments to evaluate key process parameters, and the findings are discussed in the context of microstructural characteristics and performance metrics.

Grey iron castings, such as HT250, have a composition typically including 2.5–4.0% C, 1.0–1.3% Si, 0.9–1.3% Mn, 0.3% P, 0.15% S, and balance Fe. The graphite flakes within these grey iron castings create a heterogeneous surface that can interfere with phosphate nucleation and growth. Prior investigations revealed that high-temperature manganese phosphating yields block-like, densely packed films with good corrosion resistance, while medium-temperature zinc phosphating produces flaky, incomplete films with poor performance. The medium-temperature zinc-calcium-manganese system generates granular films, but their lack of denseness compromises corrosion resistance. A fine and dense microstructure is crucial for optimal protective properties in phosphating of grey iron castings. Thus, this work seeks to refine the zinc-calcium-manganese process through parameter optimization to attain such a microstructure.

The phosphating solution was formulated with 32 g/L Zn(NO3)2, 10 g/L Ca(H2PO4)2, 9.5 g/L acid manganese phosphate, and 1 g/L tartaric acid. The bath temperature was maintained at 70–80°C. Substrates of HT250 grey iron castings, sized 50 mm × 10 mm × 5 mm, were prepared by grinding with 240-grit and 400-grit sandpaper, followed by degreasing with a phosphate-free cleaner at room temperature for 5 minutes and pickling in 50 g/L phosphoric acid at room temperature to remove rust. After rinsing with flowing tap water for 1 minute, the samples underwent phosphating under varying conditions.

An orthogonal experimental design, specifically an L16(410) array, was employed to investigate four factors: total acid (TA) at 20, 30, 40, and 50 points; acid ratio (TA/FA) at 6.6, 10.0, 14.0, and 18.0; pickling time at 20, 30, 40, and 50 seconds; and phosphating time at 5, 10, 15, and 20 minutes. The corrosion resistance of the phosphate films was assessed via a drop test according to QB/T 3824-1999, using a solution of 0.25 mol/L CuSO4·5H2O, 10% NaCl, and 0.1 mol/L HCl in a volume ratio of 40.0:20.0:0.8. The time for red rust spots to appear at 25 ± 2°C was recorded, with longer times indicating better corrosion resistance. Surface morphology was examined using scanning electron microscopy (SEM).

The orthogonal experiment results are summarized in Table 1, which presents the drop test times for each trial. To analyze the influence of each factor, the range (R) and mean effects were calculated. The range analysis indicates the order of factor impact on corrosion resistance: acid ratio > phosphating time > total acid > pickling time. This suggests that controlling the acid ratio and phosphating time is critical for optimizing the phosphating of grey iron castings. Variance analysis further confirmed no significant interaction between total acid and acid ratio, simplifying the optimization process.

Experiment No. Total Acid (Points) Acid Ratio (TA/FA) Pickling Time (s) Phosphating Time (min) Drop Test Time (s)
1 20 18.0 20 5 61
2 20 14.0 30 10 35
3 20 10.0 40 15 24
4 20 6.6 50 20 20
5 30 18.0 40 20 445
6 30 14.0 50 15 937
7 30 10.0 20 10 90
8 30 6.6 30 5 25
9 40 18.0 50 10 572
10 40 14.0 40 5 70
11 40 10.0 30 20 324
12 40 6.6 20 15 69
13 50 18.0 30 15 80
14 50 14.0 20 20 280
15 50 10.0 50 5 30
16 50 6.6 40 10 40

The effect of each parameter on corrosion resistance is discussed in detail. Total acid (TA) represents the concentration of phosphate ions in the solution. Higher TA increases the availability of phosphate species for deposition, promoting faster film formation and denser layers. However, excessively high TA can lead to coarse crystals and incorporated impurities, reducing film quality. As shown in Figure 1, derived from the orthogonal data, the optimal TA for grey iron castings is 30 points, where drop test times peak. This balance ensures sufficient nucleation sites without excessive grain growth.

$$ \text{Effect of TA} = \frac{\sum \text{Drop time at TA level}}{\text{Number of trials}} $$

For TA = 20 points: (61+35+24+20)/4 = 35.0 s; TA = 30 points: (445+937+90+25)/4 = 374.3 s; TA = 40 points: (572+70+324+69)/4 = 258.8 s; TA = 50 points: (80+280+30+40)/4 = 107.5 s. Thus, the maximum average drop time occurs at TA = 30 points.

Acid ratio (TA/FA) controls the balance between total and free acid, influencing the pH at the metal-solution interface. A higher acid ratio (lower free acid) slows hydrogen evolution on cathodic sites, allowing gradual pH rise and fine crystal formation. Conversely, a low acid ratio (high free acid) accelerates hydrogen bubble formation, disrupting deposition and causing porous films. Figure 2 illustrates that an acid ratio of 14.0 yields the best corrosion resistance for grey iron castings, as it optimizes the nucleation environment.

$$ \text{Optimal Acid Ratio} = \arg\max_{\text{TA/FA}} \left( \text{Drop Time} \right) $$

From the data: TA/FA = 18.0: (61+445+572+80)/4 = 289.5 s; TA/FA = 14.0: (35+937+70+280)/4 = 330.5 s; TA/FA = 10.0: (24+90+324+30)/4 = 117.0 s; TA/FA = 6.6: (20+25+69+40)/4 = 38.5 s. Hence, TA/FA = 14.0 maximizes performance.

Phosphating time affects film thickness and integrity. Longer times allow more complete coverage and thicker layers, but prolonged exposure can lead to acid attack and coarsening. Figure 3 shows that 15 minutes is optimal for grey iron castings, providing adequate time for film growth without degradation.

Pickling time in phosphoric acid prepares the surface by removing oxides. Insufficient pickling leaves barriers to adhesion, while excessive pickling exposes graphite flakes, hindering phosphate bonding. Figure 4 indicates that 30–40 seconds in 50 g/L H3PO4 is suitable for grey iron castings, balancing oxide removal and substrate preservation.

To correlate microstructure with performance, SEM analysis was conducted on four samples with varying corrosion resistance, prepared under conditions listed in Table 2. The micrographs reveal distinct crystal morphologies. Sample with TA 30 points, acid ratio 14.0, pickling 50 s, and phosphating 15 min (drop time 937 s) exhibits flat, block-like crystals 2–3 μm in size, densely packed into a uniform film. Sample with TA 40 points, acid ratio 18.0, pickling 50 s, phosphating 10 min (572 s) shows feathery and flaky crystals 4–5 μm, interlocked but less dense. Sample with TA 40 points, acid ratio 10.0, pickling 30 s, phosphating 20 min (324 s) has rectangular blocks 1–2 μm, loosely stacked with pores. Sample with TA 50 points, acid ratio 6.6, pickling 40 s, phosphating 10 min (40 s) displays irregular rounded particles 0.5–3.0 μm, forming a porous, uneven layer. This confirms that fine, uniform, and tightly packed crystals are essential for high corrosion resistance in phosphating of grey iron castings.

Total Acid (Points) Acid Ratio (TA/FA) Pickling Time (s) Phosphating Time (min) Corrosion Resistance Drop Test Time (s)
30 14.0 50 15 Excellent 937
40 18.0 50 10 Good 572
40 10.0 30 20 Moderate 324
50 6.6 40 10 Poor 40

The phosphating mechanism involves electrochemical reactions at the metal-solution interface. For grey iron castings, the process can be described by simplified equations. The dissolution of iron in acidic medium: $$ \text{Fe} + 2\text{H}^+ \rightarrow \text{Fe}^{2+} + \text{H}_2 \uparrow $$ The hydrolysis of primary phosphates: $$ 3\text{Zn(H}_2\text{PO}_4)_2 \rightarrow \text{Zn}_3(\text{PO}_4)_2 + 4\text{H}_3\text{PO}_4 $$ The precipitation of hopeite (zinc phosphate) and other phases: $$ 3\text{Zn}^{2+} + 2\text{H}_2\text{PO}_4^- \rightarrow \text{Zn}_3(\text{PO}_4)_2 + 4\text{H}^+ $$ In the presence of calcium and manganese, mixed phosphate films form, enhancing density and corrosion resistance. The optimal parameters promote these reactions uniformly across the heterogeneous surface of grey iron castings.

Industrial implications are significant. The optimized medium-temperature zinc-calcium-manganese process offers energy savings compared to high-temperature systems, while addressing the unique challenges of grey iron castings. By achieving a fine-grained, dense phosphate layer, this process can improve the durability of engine components and other grey iron castings in corrosive environments. Future work could explore additive effects, such as accelerators or stabilizers, to further enhance performance for grey iron castings.

In conclusion, the orthogonal experiment revealed that acid ratio has the greatest influence on corrosion resistance, followed by phosphating time, total acid, and pickling time. The best phosphating conditions for HT250 grey iron castings are: total acid 30 points, acid ratio 14.0, pickling time 30–40 seconds in 50 g/L phosphoric acid, and phosphating time 15 minutes at 70–80°C. This yields a phosphate film with fine, uniform crystals and dense packing, resulting in excellent corrosion resistance. These findings provide a practical guideline for surface treatment of grey iron castings in industrial applications, ensuring enhanced protection and longevity.