In the production of high-integrity steel castings for critical applications, the formation of internal defects, particularly blowholes, remains a significant challenge that compromises mechanical properties and structural reliability. This issue is especially pronounced in low-carbon alloy steel castings where traditional foundry practices may not adequately address the material’s specific solidification and gas evolution behaviors. The following analysis details a systematic quality improvement journey focused on resolving persistent blowhole defects in a specific grade, G10MnMoV6-3, by employing fundamental quality tools and a deep dive into process metallurgy. This account is presented from a first-person perspective as the lead engineer coordinating the technical response.

The component in question was a structurally critical casting with approximate dimensions of 700 mm x 360 mm x 140 mm and a maximum wall thickness of 50 mm. The material specification was G10MnMoV6-3 according to EN 10293-2015. The stringent requirements for these steel castings are summarized below:
| Parameter | Specification / Requirement |
|---|---|
| Chemical Composition (wB /%) | C ≤ 0.12; Mn: 1.20-1.80; Si ≤ 0.60; P ≤ 0.025; S ≤ 0.02; Mo: 0.20-0.40; V: 0.05-0.10; Cr ≤ 0.30; Ni ≤ 0.40; Cu ≤ 0.30 |
| Mechanical Properties | Tensile Strength (Rm): 600-750 MPa; Yield Strength (ReL): ≥ 500 MPa; Elongation (A): ≥ 18%; Impact Energy Akv (-20°C): ≥ 27 J |
| Non-Destructive Testing (NDT) | 100% Magnetic Particle Inspection (MPI) on all surfaces. 100% Ultrasonic Testing (UT) after rough machining with strict acceptance criteria (e.g., Φ3 mm or Φ1.5 mm equivalent flaw size depending on zone). Radiographic Testing (RT) to ASTM E446/E186 Level 2 or better in critical zones. |
Initial production trials using conventional melting and deoxidation practices—involving preliminary deoxidation with ferrosilicon and ferromanganese, followed by final deoxidation with aluminum ingot during tapping—resulted in an unacceptable rejection rate. Approximately 60% of castings exhibited blowhole defects upon rough machining in specific, thick-section locations (labeled A, B, and C in the original study). In severe cases, subsurface porosity was extensive. Spectrographic analysis of a badly affected casting revealed abnormally high levels of dissolved gases, particularly nitrogen and oxygen, confirming that gas porosity was the root cause.
To tackle this persistent issue, a cross-functional team was formed. Our first action was to employ a Cause-and-Effect Diagram (Ishikawa or Fishbone diagram) to structurally brainstorm all potential factors contributing to blowhole formation in these G10MnMoV6-3 steel castings. We categorized potential causes under the 5M1E headings: Man, Machine, Material, Method, Measurement, and Environment.
| Category (6M) | Potential Causes Identified |
|---|---|
| Material (Charge) | Use of high-carbon ferroalloys reducing final C content; moisture in alloys/slag formers; high gas content in scrap. |
| Method (Process) | Insufficient deoxidation practice; low pouring temperature; inadequate gating/risering design; incorrect slag cover. |
| Machine (Equipment) | Furnace lining condition promoting nitrogen pickup; inefficient degassing equipment. |
| Man (Operation) | Inconsistent tapping/deoxidation procedure; delays during pouring. |
| Measurement (Control) | Inaccurate temperature measurement; delayed or inaccurate gas analysis. |
| Environment | High humidity in the foundry atmosphere. |
The team then systematically investigated each “twig” on the fishbone diagram. A critical piece of metallurgical theory guided our analysis of the “Material” and “Method” branches. The solubility of gases like nitrogen in liquid steel is influenced by alloy composition and temperature. For nitrogen, a simplified solubility product at 1873 K (1600°C) and 1 atm can be expressed as:
$$ \log[\%N] = -\frac{188}{T} – 1.25 + \sum (e_N^j \cdot [\%j]) $$
Where $e_N^j$ is the interaction parameter of element $j$ on nitrogen. More pragmatically, the equilibrium nitrogen content can be approximated by an empirical relationship that highlights the strong effects of certain elements:
$$ [N] \approx K – a_C[C] – a_{Mn}[Mn] … + a_{V}[V] + a_{Cr}[Cr] $$
Where $K$ is a constant and $a_i$ are coefficients. This relationship clearly shows that elements like Titanium, Aluminum, Vanadium, and Niobium have a strong affinity for nitrogen, forming stable nitrides and thus reducing soluble nitrogen. Crucially, carbon also has a significant negative coefficient, meaning increasing carbon content actively reduces the solubility of nitrogen in the melt. For our G10MnMoV6-3 steel castings, with a maximum carbon specification of 0.12%, the initial practice of aiming for the lower end of the range (around 0.07-0.08%) to ensure toughness was inadvertently maximizing nitrogen solubility potential.
Simultaneously, we analyzed the high oxygen content. Traditional aluminum “kill” deoxidation, while powerful, can lead to the formation of clustered alumina inclusions that may act as nuclei for gas bubble formation if the deoxidation sequence and stirring are not optimal. The reaction is:
$$ 2[Al] + 3[O] \rightarrow Al_2O_3_{(s)} \quad \Delta G^\circ = -RT \ln K_{Al} $$
Where the equilibrium constant $K_{Al} = \frac{1}{a_{[Al]}^2 \cdot a_{[O]}^3}$. Incomplete deoxidation leaves residual dissolved oxygen, which can combine with carbon during solidification to form CO gas bubbles (the carbon-oxygen reaction):
$$ [C] + [O] \rightarrow CO_{(g)} \quad \Delta G^\circ = -RT \ln K_{CO} $$
$$ K_{CO} = \frac{P_{CO}}{a_{[C]} \cdot a_{[O]}} $$
If the product $[\%C] \cdot [\%O]$ exceeds the equilibrium value for the local pressure and temperature, CO bubble formation is thermodynamically favored, leading to blowholes in the final steel castings.
Through controlled trials and data analysis, we confirmed three primary root causes from the multitude of initial possibilities, as shown below:
| # | Root Cause | Confirmation Method & Evidence | Impact on Gas Porosity |
|---|---|---|---|
| 1 | Sub-optimal Carbon Content Aiming for low C (~0.07%) |
Data correlation: Batches with C ≤ 0.08% showed ~60% defect rate. Thermodynamic analysis confirms higher N solubility. | Increases nitrogen solubility potential, raising $[N]_{eq}$. Lowers carbon available for later CO formation but increases risk from N2. |
| 2 | Inadequate Deoxidation Leading to High Oxygen Residual [O] ≥ 100 ppm |
Direct measurement from defective castings. Calculated $[\%C] \cdot [\%O]$ product was above the critical threshold for CO formation. | Directly provides reactant for CO bubble formation during solidification. Promotes oxide inclusion networks. |
| 3 | Insufficient Pouring Temperature Tpour ≤ 1570°C |
Process log review. Lower temperature reduces fluidity, hindering bubble flotation and escape from the mushy zone. | Increases viscosity, reduces gas diffusion coefficients, and shortens the time available for bubbles to rise and vent. |
Based on this root cause analysis, we developed and implemented a comprehensive countermeasure plan targeting each primary factor. The goal was to shift the process window to minimize gas solubility, maximize gas removal, and improve casting soundness without compromising other properties of the steel castings.
| Targeted Root Cause | Implemented Countermeasure | Metallurgical/Process Rationale | Target Parameter |
|---|---|---|---|
| Low Carbon Content | Charge calculation to aim for the upper specification limit. Replace high-carbon ferromanganese with electrolytic manganese for Mn adjustment. | Maximizes the beneficial effect of carbon in reducing nitrogen solubility ($-a_C[C]$ term). Eliminates carbon “burn-off” uncertainty from FeMn addition. Formula: Target [C] = 0.10 – 0.12%. | 0.10% ≤ [C] ≤ 0.12% |
| High Oxygen Content | 1. Introduce argon bubbling through a porous plug in the furnace/ladle bottom. 2. Replace aluminum ingot final deoxidation with a stream-inoculated complex deoxidizer (e.g., Ca-Si-Al based). |
1. Argon stirring promotes homogenization, flotation of inclusions, and degassing via the partial pressure dilution effect (Sievert’s Law: $[H] or [N] \propto \sqrt{P_{gas}}$). 2. Complex deoxidizer forms liquid or globular oxy-sulfides instead of solid Al2O3 clusters, which are more easily removed. Also provides mild inoculating effect. |
[O] ≤ 60 ppm |
| Low Pouring Temperature | Increase and tightly control the pouring temperature range. | Higher superheat improves metal fluidity (η decreases), increases gas diffusion rates (D increases), and extends the time for bubble flotation (Stokes’ Law: $v = \frac{2 g r^2 (\rho_m – \rho_g)}{9 \eta}$). | Tpour = 1590 ± 10 °C |
The implementation of these integrated measures yielded dramatic improvements in the quality of the produced steel castings. Statistical process control data from the first ten heats after full implementation was compelling. The carbon content was successfully maintained within the new target band. The pouring temperature demonstrated significantly reduced variability around the new, higher set point. Most importantly, ladle analysis showed that dissolved oxygen content was consistently brought below the 60 ppm threshold.
The ultimate validation came from the non-destructive evaluation of the finished components. The occurrence of blowhole defects at the previously problematic A, B, and C locations after rough machining plummeted from the initial 60% rate to less than 10%. Furthermore, the severe, widespread porosity was entirely eliminated. All steel castings from the optimized process passed the stringent ultrasonic and radiographic inspection criteria, confirming a sound internal structure.
| Process Metric / Result | Initial State (Before Improvement) | Optimized State (After Improvement) | Improvement / Comment |
|---|---|---|---|
| Aim Carbon Content [C] % | ~0.07 – 0.08 | 0.10 – 0.12 | Targeted upper spec limit |
| Pouring Temperature (°C) | ≤ 1570 (Variable) | 1590 ± 10 | Increased and tightly controlled |
| Ladle [O] Content (ppm) | ≥ 100 | ≤ 60 | Effective deoxidation & stirring |
| Blowhole Defect Rate (Loc. A,B,C) | ~60% | < 10% | Over 80% reduction in rejection |
| Severe Macro-porosity | Present | Absent | Critical issue resolved |
| UT/RT Pass Rate | Low (< 40% for first article) | ~100% (for controlled process) | Meets all NDT specifications |
This case study underscores several critical conclusions for the manufacture of high-quality, low-carbon alloy steel castings. First, a holistic view of composition is vital. For G10MnMoV6-3 and similar grades, maximizing the carbon content within specification is not merely a chemical compliance exercise but a potent metallurgical lever to control nitrogen solubility, as described by $[N]_{eq} = f([C], [Mn], [V]…)$. Second, effective gas and inclusion control requires a multi-stage approach. Combining effective argon stirring for flotation and partial pressure reduction with a stream-inoculated complex deoxidation proved far superior to simple aluminum killing for achieving low, stable oxygen levels and clean metal. The reaction kinetics and inclusion morphology are fundamentally improved. Third, sufficient superheat is a critical process parameter that cannot be compromised in the pursuit of other goals; it is essential for ensuring the fluid dynamics necessary for defect-free solidification of complex steel castings.
Most significantly, this exercise reaffirmed the immense value of structured quality tools in solving complex foundry problems. The Cause-and-Effect Diagram provided the essential framework for a comprehensive, team-based brainstorming session, preventing a narrow, symptomatic fix. By forcing a systematic exploration of all 5M1E categories, it led us to investigate fundamental metallurgical principles—expressed through relationships like the nitrogen solubility equation and the carbon-oxygen equilibrium product—that were the true keys to the solution. This methodology transformed the problem from a persistent “quality headache” into a quantifiable engineering project with clear root causes, measurable countermeasures, and verifiable results. For any organization producing demanding steel castings, cultivating the discipline to collect robust process data and the skill to apply such fundamental quality and metallurgical analysis is indispensable for achieving and sustaining world-class quality levels.