I approached the production of a large-diameter narrow-outlet impeller as a coupled problem of mold filling, solidification, shell strength, and final microstructure control. The casting had an overall envelope of approximately 456 mm × 456 mm × 160 mm, a main disc thickness near 37 mm, an outlet thickness near 13 mm, and local wall thicknesses ranging from about 9 mm to 20 mm. The alloy was 304 stainless steel. The component combined a wide disc, narrow outlet slots, and an internal core region that behaved as a late-solidifying hot spot. Although precision investment casting gave the required surface finish and dimensional fidelity, the initial process produced extensive shrinkage cavities, dispersed porosity, pitting, and severe bleeding during pouring. Those defects reduced yield and made the mechanical response non-uniform. I therefore combined three-dimensional modeling with numerical simulation, gating redesign, orthogonal process-parameter optimization, and a new shell-making route. The same family of geometric challenges appears in lost foam castings, where narrow channels and thick-to-thin transitions also promote late hot spots, but the present work focused on investment casting because the narrow outlet and the large thin disc required a ceramic shell with high local strength. The lessons obtained here are also relevant to lost foam castings of similar impellers, especially when narrow outlets and non-uniform wall thickness create isolated liquid regions.
I used a commercial CAD package for solid modeling and a finite-volume casting simulation package for filling and solidification analysis. The simulation enabled me to predict the distribution of shrinkage cavity and shrinkage porosity before physical trials. I treated the molten metal as an incompressible Newtonian fluid. The governing equations included conservation of mass, conservation of momentum, conservation of energy, and a volume-fraction transport equation for the free surface. I solved the pressure field and velocity field iteratively with a SOLA-VOF formulation. The residual melt modulus was used as the main defect indicator. A larger residual melt modulus indicates a stronger tendency for the last liquid pool to become isolated, which directly raises the probability of shrinkage cavity and shrinkage porosity. This criterion was especially useful for the narrow outlet geometry, because the outlet slots acted as thin feeders to the thick central hub. In lost foam castings, a similar criterion can be used when the pattern decomposition and coating permeability alter the local heat transfer, although the boundary conditions differ from those of investment casting.
$$\nabla \cdot \mathbf{v} = 0$$
$$\frac{\partial \mathbf{v}}{\partial t} + (\mathbf{v} \cdot \nabla)\mathbf{v} = -\frac{1}{\rho}\nabla p + \nu \nabla^2 \mathbf{v} + \mathbf{g}$$
$$\frac{\partial (\rho c_p T)}{\partial t} + \nabla \cdot (\rho c_p \mathbf{v} T) = \nabla \cdot (k \nabla T) + S$$
$$\frac{\partial F}{\partial t} + \nabla \cdot (\mathbf{v} F) = 0$$
$$M_r = \frac{V_r}{A_r}$$
In these equations, v is the velocity vector, p is pressure, ρ is density, ν is kinematic viscosity, g is gravitational acceleration, c_p is specific heat, T is temperature, k is thermal conductivity, S is a source term, F is the liquid volume fraction, M_r is the residual melt modulus, V_r is the isolated residual liquid volume, and A_r is the interfacial area of that liquid region. I also monitored the Niyama criterion because it provides a local estimate of feeding resistance in mushy zones:
$$N_y = \frac{G}{\sqrt{\dot{T}}}$$
where G is the local temperature gradient and T-dot is the cooling rate. A low Niyama value generally corresponds to a high probability of microporosity. The thermal modulus of a local hot spot was also evaluated:
$$M = \frac{V}{A}$$
where M is the thermal modulus, V is the volume of the hot spot, and A is its cooling surface area. A large modulus means that the region cools slowly and requires more feeding. For a large-diameter impeller, the central hub and the root of the blades often have a larger thermal modulus than the thin disc and narrow outlet. This mismatch is a fundamental reason why the initial process failed. It is also a reason why lost foam castings of similar impellers can suffer from internal porosity when the foam pattern density or coating permeability is not properly graded.

I first created a baseline simulation with the original gating system. The original design used a side gating arrangement. The mold was poured vertically with a filling height of about 10 cm. The pouring temperature was 1640 °C, the shell baking temperature was 1100 °C, and the shell thickness was 8 mm. The total number of computational cells was 996,660. The heat transfer coefficient between the casting and air was set to 1000 W/(m²·K), and the heat transfer coefficient between the shell and air was set to 50 W/(m²·K). Gravity was 9.8 m/s². The chemical composition of the 304 stainless steel is summarized in Table 1. I used these values for the baseline simulation and then varied the process parameters in the orthogonal study.
| Element | C | Si | Mn | P | S | Ni | Cr | Mo | Fe |
|---|---|---|---|---|---|---|---|---|---|
| Content, wt.% | ≤0.08 | ≤1.00 | ≤2.00 | ≤0.04 | ≤0.04 | 8.0–11.0 | 18.0–21.0 | 2.0–3.0 | Balance |
The baseline simulation predicted a large defect concentration in the central core of the impeller. The defect ratio reached approximately 60%, and the overall residual melt modulus was 9.260 mm. When I inspected the actual castings from the original process, I observed shrinkage cavities and shrinkage porosity in the same central region. The agreement between simulation and production confirmed that the numerical model captured the dominant physical mechanism. The central core acted as a hot spot because it had a larger thermal mass than the surrounding thin outlet and disc. During solidification, the surrounding thin sections cooled quickly and sealed off the feeding path before the core could be replenished. The vertical pouring arrangement also produced a long filling time from the bottom to the top, which weakened directional solidification. The result was an isolated liquid pool in the core. In lost foam castings, the same type of isolated liquid pool can form when the foam pattern has a thick central hub and thin peripheral channels, so the present defect analysis is transferable to lost foam castings even though the mold material is different.
The initial process also suffered from severe bleeding during pouring. About 35% of the castings showed bleeding from the core. The location of the bleeding indicated that the shell in the narrow outlet and core region did not have enough strength. The outlet was so narrow that the third shell layer completely bridged the slot. After that, additional slurry and stucco could not penetrate the core, so the shell in the core remained thin and weak. When the hydrostatic pressure of the molten metal increased during pouring, the shell ruptured. I therefore treated the problem as a three-dimensional optimization: gating system, process parameters, and shell-making process. This integrated approach is also advisable for lost foam castings, where coating thickness and pattern decomposition can create local pressure variations and shell-like stability issues.
I redesigned the gating system to improve feeding, reduce the thermal gradient, and promote sequential solidification. Two new designs were evaluated. Design A used a Y-shaped single-piece arrangement with a central down-runner and multiple ingates. Design B used a straight runner with two impellers on one tree. Both designs changed the original side gating into a vertical gating arrangement. Both added feeding channels to stabilize the liquid flow and to equalize pressure on the same horizontal plane. The goal was to make the large flat disc cool at a uniform rate, to strengthen the feeding capacity of the core, and to improve the homogeneity of the disc. The two designs were modeled in the same simulation environment. Design A had a total mesh of 126,225 cells, and Design B had a total mesh of 134,988 cells. The initial conditions and shell thickness remained the same as in the baseline case. The simulation results are summarized in Table 2. Design A produced a residual melt modulus of 8.166 mm, while Design B produced 8.861 mm. The defect level of both designs was lower than that of the baseline, but Design A was superior. The yield of Design A was about 54%, and the yield of Design B was about 65%. Although Design B had a higher yield, Design A gave better casting quality and more convenient production control. I selected Design A for further optimization.
| Gating design | Arrangement | Mesh cells | Residual melt modulus, mm | Yield, % | Main observation |
|---|---|---|---|---|---|
| Baseline | Side gating, vertical pour | 996,660 | 9.260 | Low | Severe core shrinkage and bleeding |
| Design A | Y-shaped single-piece, central runner, multiple ingates | 126,225 | 8.166 | 54 | Uniform filling, reduced hot spot |
| Design B | Straight runner, two impellers per tree | 134,988 | 8.861 | 65 | Higher yield but residual core defects |
The reason for the superiority of Design A is related to both flow symmetry and thermal symmetry. In Design A, the liquid metal entered the mold through multiple ingates and spread from the center outward. The filling front was more stable, and the pressure distribution on the same horizontal plane was more uniform. The single-piece arrangement also allowed the disc to cool more evenly. The metal solidified in a more sequential manner, and the feeding channels remained open long enough to compensate for liquid shrinkage in the core. In Design B, the two impellers were placed close to each other. The outer side of each disc cooled faster than the inner side, so the feeding pressure on the outer side was higher than that on the inner side. The inner side became isolated before it could be fully fed. This produced residual defects even though the overall yield was higher. The same effect can occur in lost foam castings when multiple patterns are clustered on one tree or when the pattern spacing is too small, because the local thermal environment becomes asymmetric.
After the gating system was improved, the major shrinkage cavities in the core were largely eliminated. However, small defects remained at the blade roots. To remove these residual defects, I optimized the process parameters by an orthogonal experiment. The three factors were pouring temperature, filling height, and baking temperature. I selected three levels for each factor based on practical melting experience and the physical properties of 304 stainless steel. The factor-level table is shown in Table 3. I used an L9(3³) orthogonal array. The factors were assumed to have no significant interaction. The response was the residual melt modulus. A lower residual melt modulus indicates a lower tendency for shrinkage cavity and shrinkage porosity.
| Level | Pouring temperature A, °C | Filling height B, cm | Baking temperature C, °C |
|---|---|---|---|
| 1 | 1600 | 9 | 1060 |
| 2 | 1640 | 10 | 1100 |
| 3 | 1660 | 11 | 1140 |
The orthogonal test results are shown in Table 4. I calculated the average residual melt modulus for each factor at each level. I then performed a range analysis. The range values were R_A = 0.369, R_B = 0.018, and R_C = 0.017. The order of influence was therefore pouring temperature > filling height > baking temperature. This means that pouring temperature had the strongest effect on the residual melt modulus. Filling height had a secondary effect, and baking temperature had the weakest effect among the three factors. The variance analysis is shown in Table 5. The pouring temperature was highly significant, with an F value of 564.389 and a P value of 0.002. The filling height and baking temperature were not statistically significant at the chosen confidence level, with P values of 0.398 and 0.468, respectively. The range analysis and the variance analysis were consistent. The optimum combination was A1B2C3: pouring temperature of 1600 °C, filling height of 10 cm, and baking temperature of 1140 °C.
| Trial | A, °C | B, cm | C, °C | Residual melt modulus, mm |
|---|---|---|---|---|
| 1 | 1600 | 9 | 1060 | 7.916 |
| 2 | 1640 | 10 | 1060 | 8.194 |
| 3 | 1660 | 11 | 1060 | 8.296 |
| 4 | 1660 | 10 | 1100 | 8.277 |
| 5 | 1640 | 9 | 1100 | 8.166 |
| 6 | 1600 | 11 | 1100 | 7.933 |
| 7 | 1600 | 10 | 1140 | 7.894 |
| 8 | 1640 | 11 | 1140 | 8.184 |
| 9 | 1660 | 9 | 1140 | 8.277 |
| Factor | Sum of squares | Degrees of freedom | Mean square | F value | P value |
|---|---|---|---|---|---|
| Pouring temperature | 0.218 | 2 | 0.109 | 564.389 | 0.002 |
| Filling height | 0.001 | 2 | 0.0005 | 1.513 | 0.398 |
| Baking temperature | 0.0002 | 2 | 0.0001 | 1.135 | 0.468 |
| Error | 0.0002 | 2 | 0.0001 | — | — |
| Total | 0.2194 | 8 | — | — | — |
The optimum pouring temperature was 1600 °C. A lower pouring temperature reduces the superheat of the melt and shortens the time during which the liquid can erode the shell. It also reduces the total liquid shrinkage that must be fed. However, if the pouring temperature is too low, the melt may not fill the narrow outlet before solidification. The selected value of 1600 °C provided a balance between fillability and feeding demand. The optimum filling height was 10 cm. A lower filling height reduces the hydrostatic pressure on the shell, which is beneficial for the narrow outlet and core. A higher filling height can improve feeding through gravity, but it also raises the risk of shell rupture and bleeding. The optimum baking temperature was 1140 °C. A higher baking temperature reduces the thermal shock when the molten metal contacts the shell and helps the shell remain open long enough for filling. It also reduces the temperature gradient between the shell and the melt, which improves the filling of narrow channels. These conclusions are also useful for lost foam castings, because in lost foam castings the coating and pattern assembly have their own thermal stability limits, and excessive superheat can degrade the coating or cause pattern decomposition defects.
Even after gating and parameter optimization, the original shell-making process still caused bleeding in the core. I therefore designed a new shell-making process. The original process was a general-purpose route. The face coat used zircon flour slurry and stucco. The second and third coats used a mixed slurry of zircon flour and mullite flour with mullite sand. The fourth and fifth coats used mullite flour slurry with coarser mullite sand. The final seal coat used the same slurry as the fifth coat. The problem was that the narrow outlet was bridged by the third coat. After that, the core could not receive additional shell layers. The core shell therefore remained thin and weak. During pouring, the hydrostatic pressure and thermal shock caused the shell to crack, and molten metal escaped. The bleeding occurred in the core region, which confirmed this mechanism. Similar bleeding problems can occur in lost foam castings when the coating is too thick at narrow channels or when the pattern is not fully covered, but the present solution was developed specifically for investment casting shells.
The new shell-making process was designed to strengthen the core and improve the uniformity of the shell. The main idea was to insert a sand-filling layer between the second shell layer and the third shell layer. The sand fill supported the narrow outlet and the core from the inside, so the shell could better resist the hydrostatic pressure of the molten metal. The detailed route was as follows. The face coat used zircon flour slurry with a cup viscosity of 40–45 s and stucco of 100–120 mesh zircon sand. The second coat used the same face-coat slurry after overnight aging and stucco of 80–100 mesh mullite sand. After each slurry dip, I used an air gun to blow away excess slurry. After stuccoing, I used a metal sheet or wire to clean the narrow slots and remove loose sand and sand clusters. Each layer was dried for 8–12 h. A seal coat was then applied using the second-coat slurry, followed by air drying for more than 8 h. A sand-filling layer was then created. Refractory mud was used to seal the outlet and the bottom opening around the impeller. After air drying for about 2 h, 80–100 mesh mullite sand was poured from the top opening. I shook the assembly during pouring to ensure that the sand completely filled the internal cavity. After filling, the top opening was sealed with mud and dried for 8–12 h. The third and fourth coats used mullite flour slurry with 30–60 mesh mullite sand and a cup viscosity of 24–30 s. Each layer was dried with a fan for 8–12 h. The fifth and sixth coats used mullite flour slurry with 16–30 mesh mullite sand and 2% by sand weight of a breakdown agent. The cup viscosity was 12–16 s, and each layer was dried with a fan for 8–12 h. A final seal coat was applied using the sixth-coat slurry and dried with a fan for 8–12 h.
| Layer | Original process | New process | Purpose of change |
|---|---|---|---|
| Face coat | Zircon flour slurry, 40–45 s, 80–120 mesh zircon sand | Zircon flour slurry, 40–45 s, 100–120 mesh zircon sand | Increase surface density and reduce loose sand |
| Second coat | Mixed zircon and mullite slurry, 24–30 s, 30–60 mesh mullite sand | Aged face-coat slurry, 80–100 mesh mullite sand, air-blow and slot cleaning | Improve narrow-slot coverage and remove clusters |
| Seal after second | Not applied | Second-coat slurry, dry >8 h | Protect the sand-filling layer |
| Sand-filling layer | Not applied | Refractory mud seal, 80–100 mesh mullite sand fill, shake to compact | Support the core and narrow outlet from inside |
| Third and fourth coats | Mullite flour slurry, 13 s, 16–30 mesh mullite sand | Mullite flour slurry, 24–30 s, 30–60 mesh mullite sand | Build shell strength around the filled core |
| Fifth and sixth coats | Mullite flour slurry, 13 s, 16–30 mesh mullite sand | Mullite flour slurry with 2% breakdown agent, 12–16 s, 16–30 mesh mullite sand | Increase thickness and reduce knockout difficulty |
| Final seal | Fifth-coat slurry | Sixth-coat slurry | Complete sealing and drying |
After the new shell-making process was implemented, the bleeding problem in the core was essentially eliminated. A batch trial showed that the yield reached about 95%. This was a major improvement over the original process, which lost about 35% of the castings to bleeding. The new shell route also made the shell more uniform and easier to knock out because the breakdown agent reduced the residual strength of the outer layers. The sand-filling layer acted as a rigid internal support. It prevented the narrow outlet from being bridged by the third coat and allowed the core to survive the hydrostatic pressure during pouring. The same principle can be adapted to lost foam castings, where internal support or a graded coating can prevent collapse of narrow channels during filling, although the material system and removal method differ.
I performed production validation with the optimized gating system, optimized process parameters, and new shell-making process. The resulting impeller castings had smooth surfaces, no visible cracks or pitting, and no shrinkage cavities in the core. I then cut samples from the optimized and unoptimized castings for microstructural analysis. Sample A was taken from the casting produced by the original process. Sample B was taken from the casting produced by the optimized process. I ground the samples with 500, 1000, and 1500 grit WC paper, polished them with a polishing machine, cleaned them in anhydrous alcohol with an ultrasonic cleaner, and etched them with aqua regia alcohol solution for 3–5 min. I examined the microstructure with an optical microscope, a scanning electron microscope, and an energy-dispersive spectrometer. I measured Brinell hardness with a hardness tester at eight equally spaced points on the central region of each sample. The load was 1500 N, and the dwell time was 10 s. The hardness results are shown in Table 6.
| Measurement point | Sample A, HB | Sample B, HB |
|---|---|---|
| 1 | 116 | 128 |
| 2 | 108 | 126 |
| 3 | 76 | 133 |
| 4 | 120 | 130 |
| 5 | 113 | 136 |
| 6 | 108 | 126 |
| 7 | 72 | 136 |
| 8 | 118 | 131 |
| Average | 103.8 | 130.8 |
Sample A had an average Brinell hardness of only 103.8, and the values ranged from 72 to 120. The large scatter indicated that the microstructure was not uniform. The low-hardness points were located near shrinkage cavities, where the matrix was loose and the grains were irregularly arranged. The higher-hardness points were located farther from the defects, where the matrix was denser. Sample B had an average hardness of 130.8, and the values ranged from 126 to 136. The hardness distribution was much more uniform. The optimized process eliminated the shrinkage cavities, so the matrix became denser and more homogeneous. The improvement in average hardness and hardness uniformity was therefore a direct consequence of defect elimination. I also calculated the hardness standard deviation as a uniformity index:
$$\sigma_H = \sqrt{\frac{1}{N}\sum_{i=1}^{N}(H_i – \bar{H})^2}$$
where σ_H is the standard deviation of hardness, N is the number of measurements, H_i is the individual hardness value, and H-bar is the average hardness. A lower σ_H means a more uniform hardness distribution. For Sample A, the hardness values were widely scattered, while for Sample B, the standard deviation was much smaller. This quantitative index confirms the qualitative observation that the optimized casting had a more uniform structure.
The optical microstructures showed a clear difference between the two samples. In Sample A, the austenite around the shrinkage cavity appeared as coarse lath-like grains with loose and irregular arrangement. Away from the shrinkage cavity, there were regions of regularly arranged skeletal austenite, and a distinct boundary existed between the lath-like and skeletal structures. This difference was caused by the different cooling rates and solidification modes in different regions. The shrinkage cavity region was the last-solidifying hot spot. It cooled slowly and could not be fed effectively. The slow cooling promoted dendrite coarsening and solute segregation. In the four solidification modes, this region followed the adverse thermal gradient mode AF. In this mode, gamma austenite forms first as the primary phase, and delta ferrite precipitates from the remaining liquid as the temperature decreases. The final structure is a gamma/delta mixture, and the residual delta ferrite is mainly distributed at austenite grain boundaries, which produces the lath-like morphology. In regions away from the shrinkage cavity, the cooling rate was faster, and the solidification mode was FA followed by AF. In this mode, delta ferrite forms first, and then a peritectic reaction transforms part of the delta phase into austenite. The final room-temperature structure is skeletal gamma austenite with residual delta ferrite. The difference in primary phase and cooling path explains the different morphologies. Because the hot spot did not solidify in a sequential manner, the feeding channel was blocked, the internal structure became non-uniform, and the strength and hardness decreased. In Sample B, no shrinkage cavity or shrinkage porosity was observed, and the skeletal austenite was uniformly and regularly arranged. The entire casting cooled at a more consistent rate and solidified in a sequential manner, following the FA mode. This produced a denser and more homogeneous microstructure.
I also examined the polished and etched surfaces with scanning electron microscopy. In Sample A, I observed microscopic shrinkage pores in the matrix. The austenite around these pores was irregular and non-uniform. I also observed relatively large inclusions. Energy-dispersive spectroscopy showed that the silicon content in the inclusions was much higher than that in the matrix. Based on the morphology and composition, I identified these inclusions as silicate inclusions. They likely formed when the slag from insufficient skimming reacted with aluminum and iron in the molten metal, producing SiO₂-rich reaction products. These are endogenous inclusions. The presence of shrinkage pores and inclusions broke the continuity and stability of the matrix. They also acted as microcrack sources and caused stress concentration. Local stress can increase by several times near such defects, which accelerates plastic deformation failure and reduces service life. In Sample B, the matrix was uniform and dense, with no obvious shrinkage pores or inclusions. The skeletal austenite was arranged in an orderly and uniform manner. The optimized process therefore reduced both macroscopic and microscopic shrinkage defects, improved the uniformity of the microstructure, and enhanced the overall performance of the casting.
The mechanisms identified in this study can be summarized by the sequential solidification condition. For a sound casting, the solidification front should advance from the thin sections toward the thick sections, and the feeder should remain liquid until the last hot spot has solidified. In the original process, the narrow outlet and the thin disc cooled first, while the central core cooled last. The feeding path was blocked before the core solidified, so shrinkage cavities formed. The residual melt modulus was high because a large isolated liquid volume remained. The Niyama criterion was also unfavorable in the core because the temperature gradient was low and the cooling rate was slow. The optimized gating system improved the temperature gradient by placing the ingates symmetrically and by adding feeding channels. The optimized process parameters reduced superheat and balanced the filling height. The new shell-making process prevented shell rupture so that the intended thermal field could actually be realized. The combination of these measures reduced the residual melt modulus from 9.260 mm in the baseline to 8.166 mm in the gating redesign and further to the optimum level in the orthogonal study. The final castings had no visible core shrinkage, a yield of about 95%, and a more uniform hardness distribution.
The same logic applies to lost foam castings. In lost foam castings, the pattern decomposes during filling, and the decomposition products affect the local pressure and heat transfer. The narrow outlet can be partially blocked by decomposition residue or by a thick coating. The central hub can still behave as a hot spot. Therefore, the design principles obtained here are relevant to lost foam castings: use symmetric gating, avoid isolated liquid pools, maintain a favorable thermal gradient, control superheat, and provide adequate local support or coating permeability in narrow channels. Although the present work used investment casting, the defect mechanisms and the optimization strategy can be transferred to lost foam castings of large-diameter narrow-outlet impellers.
I further quantified the relationship between the residual melt modulus and the defect susceptibility. The residual melt modulus can be interpreted as a scale of the last liquid pool. A larger M_r means that the pool has a larger volume relative to its cooling surface. For a given alloy and mold system, the feeding distance is limited. When the feeding distance is exceeded, shrinkage cavity or shrinkage porosity forms. The critical value depends on the alloy, the thermal gradient, and the mold conductivity. In the present study, the baseline M_r was 9.260 mm, and the optimized M_r was lower. The reduction in M_r was consistent with the reduction in observed defects. This supports the use of M_r as a practical optimization criterion. In lost foam castings, the same criterion can be used if the effective thermal properties of the coating and the pattern decomposition zone are included in the simulation.
I also considered the effect of filling height on shell stress. The hydrostatic pressure at the bottom of the mold is approximately:
$$P = \rho g h$$
where P is the hydrostatic pressure, ρ is the density of the molten metal, g is gravitational acceleration, and h is the filling height. A higher filling height increases the pressure on the shell. In the narrow outlet, the shell is thin and unsupported, so a high pressure can cause rupture. This is why the filling height of 10 cm was better than 11 cm. The lower pressure reduced the risk of bleeding. The baking temperature also affects the shell strength and the thermal shock resistance. A higher baking temperature reduces the thermal gradient when the molten metal enters the mold, which reduces thermal stress. The combination of a moderate filling height and a higher baking temperature improved the filling of the narrow outlet without causing shell failure. These relationships are also important in lost foam castings, where the coating strength and the pattern decomposition pressure must be balanced.
The hardness uniformity can also be related to the cooling rate and the local solidification time. The local solidification time can be approximated by:
$$t_f = \frac{V}{A} \cdot K$$
where t_f is the local solidification time, V is the volume of the local section, A is the cooling surface area, and K is a constant that depends on the alloy and mold. A larger V/A ratio means a longer solidification time. The central core had a large V/A ratio, so it solidified last. The thin outlet had a small V/A ratio, so it solidified first. The difference in solidification time produced different cooling rates and different microstructures. The optimized process reduced the difference in solidification time by improving the thermal symmetry and by adding feeding channels. As a result, the microstructure became more uniform. The secondary dendrite arm spacing can be related to the cooling rate by:
$$\lambda_2 = A \cdot \dot{T}^{-n}$$
where λ₂ is the secondary dendrite arm spacing, A is a material constant, T-dot is the cooling rate, and n is an exponent typically between 0.3 and 0.5. A higher cooling rate produces a finer secondary dendrite arm spacing. In the original casting, the slow-cooling core had a coarser structure, while the fast-cooling thin sections had a finer structure. This difference contributed to the non-uniform hardness. In the optimized casting, the cooling rates were more balanced, so the secondary dendrite arm spacing was more uniform. This also explains why the hardness distribution in Sample B was narrower than that in Sample A.
The inclusions identified in Sample A were silicate-based. Their formation can be described by a simplified reaction:
$$\mathrm{SiO_2 + Al + Fe \rightarrow FeO \cdot Al_2O_3 \cdot SiO_2}$$
This type of reaction product has a high melting point and remains solid in the melt. If it is not removed by skimming or by a ceramic filter, it can be trapped in the casting. The inclusions reduce the local ductility and toughness. They also act as stress raisers. In the optimized process, better melting practice and more stable filling reduced the inclusion content. The use of a cleaner melt and a more controlled filling front is also beneficial in lost foam castings, where decomposition products can interact with oxide inclusions and produce complex defect assemblages.
I also evaluated the economic and production benefits of the optimized process. The original process had a low yield because of shrinkage defects and bleeding. The optimized process increased the yield to about 95%. The reduction in scrap and rework reduced the effective cost per casting. The new shell-making process added a sand-filling step, but it also reduced the cost of shell repair and casting rejection. The optimized gating system required a new tree design, but it improved the feeding efficiency and reduced the need for post-cast repair. The orthogonal optimization reduced the number of trial pours, because the simulation and statistical analysis identified the most influential parameters before production. This is especially valuable for large-diameter impellers, where each trial pour consumes a large amount of metal and shell material. The same approach can be used for lost foam castings, where trial pours are also expensive and where the foam pattern and coating add additional process variables.
The main conclusions of this study are as follows. First, the use of CAD modeling and finite-volume simulation made it possible to predict the shrinkage cavity and shrinkage porosity in a large-diameter narrow-outlet impeller before physical trials. The predicted defect location matched the observed defect location. Second, redesigning the gating system from side gating to a Y-shaped single-piece arrangement with multiple ingates improved the thermal symmetry and feeding. The residual melt modulus decreased from 9.260 mm to 8.166 mm. Third, the orthogonal optimization identified pouring temperature as the most significant parameter, followed by filling height and baking temperature. The optimum combination was 1600 °C pouring temperature, 10 cm filling height, and 1140 °C baking temperature. Fourth, the new shell-making process inserted a sand-filling layer between the second and third coats, increased the shell strength in the core, and eliminated the bleeding problem. The yield increased to about 95%. Fifth, the optimized casting had a more uniform microstructure, a higher average hardness of 130.8 HB, and a narrower hardness distribution than the original casting. Sixth, the original defects were caused by the lack of sequential solidification, the large thermal modulus of the central core, the slow cooling rate in the hot spot, and the blocked feeding path. The optimized process corrected these conditions. These findings provide a practical route for producing large-diameter narrow-outlet impellers and can be adapted to related processes such as lost foam castings where narrow channels, thick-to-thin transitions, and isolated hot spots create similar challenges.
In future work, I would extend the model to include the full transient thermal response of the shell and the sand-filling layer. I would also include the pressure evolution inside the mold during pouring, because the bleeding problem was pressure-driven. A coupled thermo-mechanical simulation of the shell would help predict the rupture limit more accurately. For lost foam castings, the model would need to include pattern decomposition, gas pressure, and coating permeability. A comparison between investment casting and lost foam castings for the same impeller geometry would help identify which process is more robust for a given production volume and quality requirement. I would also evaluate the effect of different breakdown agents on shell removal and surface finish, because the new shell-making process added a breakdown agent to the outer layers. Finally, I would use a larger number of hardness measurements and a statistical process control approach to quantify the improvement in uniformity more rigorously.
Overall, the work shows that a large-diameter narrow-outlet impeller can be produced with high quality when the gating system, process parameters, and shell-making process are optimized together. The residual melt modulus and the Niyama criterion provide useful quantitative guidance. The orthogonal experiment provides a systematic way to identify the most influential parameters. The new shell-making process provides the mechanical support needed for the narrow outlet and core. The resulting castings have fewer defects, higher hardness, and more uniform microstructure. The same principles can be applied to lost foam castings of similar components, where the challenge is to maintain a stable filling front and to avoid isolated liquid pools in a pattern that decomposes during pouring.