Quality inspection results of railway steel castings

During the trial production of coupler steel castings, the process scheme is continuously optimized and the casting quality is continuously improved. Finally, qualified coupler parts can be stably produced, which shows that the quality inspection results of coupler steel castings meet the requirements of relevant technical indexes. The quality inspection results of qualified parts obtained from trial production of hook body and hook tongue by improved and optimized process are introduced in detail.

(1) Physical and chemical properties

CSiMnPSNiCrMoCuAlAs
0.2700.3401.3500.0140.0070.3900.4800.2400.0500.0400.007

The physical and chemical performance test mainly includes the chemical composition, mechanical properties and metallographic structure of the coupler, and the test results all meet the specified requirements.

CategoryTensile strength (MPa)Yield strength (MPa)Elongation after fracture (%)Reduction of area (%)-40 ° C impact absorption energy (J)Tensile specimen (mm)
Type 17 Leptospira945855163750122×50
Type 16 hook tongue940860163531122×50
categoryType I, IIIType IIOtherMatrix structure
Type 17 LeptospiraNoneNoneNoneQuenching and tempering organization level 4
Type 16 hook tongueNoneNoneNoneQuenching and tempering organization level 4

(2) Compactness

ProfileA-AB-BC-CD-DE-EF-FG-GTail A-ATail B-BTail C-CTail D-D
Specified level≤3≤5≤4≤4≤4≤2≤4≤3≤4≤4≤3
Actual level≤1≤1≤1≤1=1≤1≤1≤1≤1≤1≤1

According to the technical standards, the coupler body and coupler tongue shall be dissected at the designated part, and the section compactness of the dissected section shall be tested. The cutting position of the coupler body and coupler tongue is shown in Figure 1. The test report of the compactness of the coupler body and coupler tongue is shown in table 4 and table 5. All the test results meet the specified requirements. The actual cutting photos of the steel castings of the coupler body and coupler tongue are shown in Figure 2.

ProfileA-AB-BC-C
Specified level≤3≤4≤2
Actual level≤1≤1≤1
(a) C-C section of 17 type hook body and hook head (b) Section B-B of type 16 knuckle

(3) Surface quality and appearance dimension

The trial produced 16 and 17 type couplers (coupler body and coupler tongue) have been checked by CMM, sample plate and anatomy. The geometric dimension and wall thickness of each part meet the requirements of steel casting drawing. Through visual inspection, the steel castings are free of cracks and shovel marks on the inner and outer surfaces, and there are no steps, cracks and core supports at important parts of the inner cavity.

(4) Hardness

The surface of the hook tongue and the end face of the hook tail shall be subject to heat treatment, and the surface of the hook tail ball shall meet the requirements of type A. The hardness test report of coupler slice is shown in table 6.

CategoryDepth from traction surface 5mm / HBWDepth from traction surface 10mm / HBWDistance from end spherical surface 4.5mm / HBW
Type 17 Leptospira429306455
Type 16 hook tongue448302406

(5) FeO content of slag sample in reduction period

The FeO content test results of slag samples in reduction period are shown in table 7.

Sample nameTest itemsStandard content /%Test content /%
SlagFeO≤10.85

(6) Dynamic tear

The dynamic tear test results meet the requirements, and the test results are shown in table 8.

Sample nameTexture of materialTest temperature / ° CDT/J
NoumenonGrade E steel-56130
Test barGrade E steel-56165

(7) Hardenability of Grade E steel

The test samples of 5 heats were selected for the hardenability test of Grade E steel. The test results meet the requirements, and the hardenability curve is shown in Figure 3.

(8) Static load tensile test

Two type 17 hooks and two type 16 tongues were randomly selected for static load tensile test. The test results meet the requirements. The test results are shown in table 9.

CategoryTechnical requirements for maximum permanent deformation / mmMaximum permanent deformation inspection result / mmTechnical requirements for minimum failure load / kNMinimum failure load test result / kN
Type 17 Leptospira≤ 0.8 when loading 3115kn0.1≥40054005 not broken
Type 16 hook tongue≤ 0.8 when loading 1780kN0.2≥34303430 not broken