Control of Slag Inclusion Defects in Automotive Steel Production

Since the second half of 2019, our cold rolling process has intermittently detected slag inclusion defects when rolling steel plates for automotive applications. In severe cases, these defects lead to batch blockages and downgrading of the material. More critically, automotive customers have reported part cracking during the stamping of various components directly attributable to these slag inclusions. In the worst scenarios, stamped parts cannot be reworked and are scrapped outright. The presence of slag inclusion defects in the continuous cast slab for automotive steel severely impacts production efficiency and quality costs. Therefore, the sustained reduction and control of slag inclusion defects has been a long-term, paramount objective in our steelmaking operations.

Morphology and Composition Analysis of Slag Inclusion

Automotive steel is typically rolled and stamped into thin parts with a final gauge of 0.5 to 1.0 mm. During this severe rolling deformation, any initial slag inclusion in the slab is elongated. On the surface of the finished part, the defect manifests as a long, linear seam running parallel to the rolling direction, which can evolve into a significant crack in serious cases.

Analysis of samples taken from customer-rejected parts involved sectioning through the defect area and preparing metallographic specimens. Scanning Electron Microscopy (SEM) with Energy Dispersive X-ray Spectroscopy (EDS) revealed the presence of fine, subsurface inclusions at the defect site. These inclusions were composed primarily of carbon, oxygen, fluorine, sodium, magnesium, aluminum, silicon, sulfur, calcium, titanium, and iron. This composition profile definitively confirms that the defect originates from a slag inclusion entrained during the steelmaking and casting process. The characteristic composition indicates the involvement of mold flux, refractory materials, and deoxidation products.

Sources and Formation Mechanism of Slab Slag Inclusion

Slag inclusion in the slab, often termed “slag entrapment” or “slag blister,” generally occurs when mold flux on the surface of the molten steel in the mold becomes embedded into the solidifying shell. This is particularly prevalent when the mold flux has a high melting point or poor fluidity. The formation of a slag inclusion defect is a complex interplay of fluid dynamics, thermal conditions, and material properties.

Primary Sources of Inclusions

For continuous cast slab, the main sources of material that lead to slag inclusion defects are categorized as follows:

  • Ladle Slag and Refractory Erosion: At the end of ladle teeming, a delayed closure of the ladle slide gate can allow ladle slag to drain into the tundish. Furthermore, erosion of tundish linings and submerged entry nozzles (SEN) contributes exogenous inclusions to the steel.
  • Mold Flux Entrapment: Sub-optimal performance of the mold powder, such as inadequate melting or the formation of a solidified crust, can lead to patches of unmelted or partially melted flux being dragged into the solidifying shell.
  • Endogenous Inclusions: These are primarily aluminum oxides (alumina clusters) formed during the deoxidation process in the ladle. If not properly floated out, they can act as nuclei for slag entrapment or be directly captured.

All these sources—ladle slag, refractory particles, and unassimilated mold flux—can become trapped at the solidification front, resulting in a slag inclusion defect.

The Process of Slag Inclusion Formation

The formation of a slag inclusion defect follows two primary modes: entrainment into the steel bulk and adhesion to the slab surface.

During casting, with the SEN positioned at the mold center, the fluid flow should ideally be symmetrical. However, turbulent flow near the SEN ports can induce vortices, especially when the mold level fluctuates. The generation of these vortices is directly linked to the stability of the meniscus. As casting speed increases, the upward flow emanating from the SEN ports intensifies the meniscus velocity and turbulence, promoting severe slag-steel emulsification. This makes it easy for liquid mold flux to be entrained into the steel bulk.

At higher casting speeds, slag entrapment is also likely near the mold narrow face. The steel flow travels up the narrow face, impacts the meniscus, and is redirected back towards the SEN along the slag-steel interface. This flow scours and thins the slag layer near the narrow face, potentially exposing bare steel. Due to interfacial tension, some flux is carried with this flow, aggregating midway between the SEN and the narrow face. Parts of this flux can then be entrained by the steel stream.

Whether entrainment occurs at the surface or within the bulk, it is fundamentally related to turbulence at the slag-steel interface. Factors exacerbating this include a misaligned SEN causing asymmetric flow (biased flow), excessive argon bubbling, and high casting speed-induced level fluctuations. Adhesion of slag primarily happens at the meniscus; slag adhering to the initial solid shell can be pressed into the subsurface during oscillation mark formation, creating a permanent slag inclusion defect.

Influencing Factors on Slab Slag Inclusion

Analyzing the slag entrainment process reveals that several key process parameters significantly influence the severity of slag inclusion defects.

1. Influence of Mold Flux Properties

The thickness of the molten flux layer and its consumption rate per ton of steel are critical for slab surface quality. An ideal molten layer thickness is 12–15 mm, with a consumption of 0.40–0.60 kg/t. The balance between flux feeding (consumption) and melting speed is paramount. Consumption is governed by viscosity, while melting speed is an intrinsic property of the flux. For automotive steels, the specific mold flux used often has higher viscosity and lower basicity compared to fluxes for other grades.

The relationship between flux consumption (Rs), viscosity (η), and casting speed (Vc) can be approximated by:
$$ R_s = k \cdot \frac{\eta^{-0.5}}{V_c} $$
where \( k \) is a constant. Both excessively low and high consumption disrupt uniform flux infiltration at the meniscus, leading to uneven heat transfer in the initial shell and promoting surface slag inclusion defects.

Table 1: Comparison of Physical Properties Between Automotive Steel Mold Flux and Standard Mold Flux
Physical Property Automotive Steel Flux Standard Flux
Melting Point (°C) 1040 – 1120 910 – 1130
Viscosity @ 1300°C (Pa·s) 0.17 – 0.45 0.09 – 0.13
Basicity (CaO/SiO₂) 0.87 – 1.18 1.1 – 1.2

2. Influence of Argon Injection into the SEN

Argon is injected through the stopper rod and/or SEN walls to prevent nozzle clogging by keeping alumina inclusions from adhering. The bubbles also help float inclusions in the mold. However, investigation of heats linked to customer complaints revealed a common thread: excessive argon flow rates. High argon injection agitates the meniscus violently, causing large level fluctuations and bubble-driven “spouting,” which dramatically increases the risk of slag entrainment and consequent slag inclusion defects.

3. Influence of Tundish Steel Temperature (Superheat)

The superheat (temperature above liquidus) of steel in the tundish affects its fluidity. Higher superheat improves fluidity and homogeneity but can negatively affect slab structure. When superheat falls below approximately 15°C, steel viscosity increases significantly. This hampers the floatation of inclusions, increasing their chance of being trapped in the solidifying slab. Furthermore, low superheat can cause nozzle clogging, prompting operators to increase argon flow or perform nozzle purging, which further disturbs the process and can introduce more inclusions. For automotive grades, maintaining a controlled superheat range of 15–40°C is crucial.

4. Influence of Mold Level Fluctuation

This is one of the most critical factors. A stable meniscus is essential. During normal operation, mold level fluctuates slightly. However, excessive fluctuations prevent unmelted flux powder or floating inclusions (like alumina) from being properly assimilated by the liquid flux layer. Instead, they can be mechanically entrapped by the oscillating shell. Empirical observations and data from complaint heats show a direct correlation: larger mold level fluctuation amplitude corresponds to a significantly higher risk of slag inclusion defect formation. The instability is often driven by casting speed changes, excessive argon, or partial nozzle clogging.

5. Influence of Casting Speed

Casting speed (or pull rate) directly governs fluid flow dynamics in the mold. Increased casting speed raises the exit velocity from the SEN ports, intensifying the upward flow and meniscus turbulence. This worsens slag entrainment. Simultaneously, the downward flow becomes stronger and penetrates deeper, reducing the chance for inclusions to float out. Frequent changes in casting speed are particularly detrimental as they create transient, unstable flow conditions that exacerbate slag inclusion defect formation. The Weber number (We), representing the ratio of inertial to surface tension forces, can be used to assess the risk of slag entrainment:
$$ We = \frac{\rho v^2 L}{\sigma} $$
where \( \rho \) is density, \( v \) is characteristic velocity at the meniscus, \( L \) is characteristic length, and \( \sigma \) is interfacial tension. A higher We indicates greater entrainment risk.

6. Influence of Submerged Entry Nozzle (SEN) Parameters

Two key SEN parameters affect slag inclusion: alignment and immersion depth.

  • SEN Alignment: Misalignment causes biased flow, where one side of the mold has stronger upward flow than the other. This creates an asymmetric, unstable meniscus with a high potential for slag entrainment and can even lead to breakouts.
  • SEN Immersion Depth: Shallow immersion leads to strong surface flow and severe slag entrainment. Excessive immersion depth deepens the flow pattern, hindering inclusion floatation. An optimal depth balances these effects.

The Reynolds number (Re) for flow in the SEN and mold indicates turbulence level:
$$ Re = \frac{\rho v D}{\mu} $$
where \( D \) is the hydraulic diameter and \( \mu \) is the dynamic viscosity. Higher Re suggests more turbulent conditions favorable for mixing but also for slag inclusion formation if uncontrolled.

Comprehensive Countermeasures to Reduce Slag Inclusion

Based on the root cause analysis, a multi-pronged improvement strategy was implemented targeting the key influencing factors.

1. Prevention of Slag Carry-Over and Optimization of Mold Flux

To prevent ladle slag from entering the tundish, the accuracy and reliability of the ladle slag detection system were enhanced. From a flux perspective, while the existing high-viscosity flux for automotive steel helped deepen the flow pattern, its melting behavior was fine-tuned. Increasing liquid flux viscosity and reducing its wettability on steel can effectively minimize entrainment. The modified flux aimed for a more stable, consistent molten layer under our specific casting conditions.

2. Precise Control of Argon Injection Flow

Collaborating with refractory suppliers, the internal structure and dimensions of the tundish upper nozzle were optimized to improve gas distribution. Rigorous maintenance of argon lines was enforced to ensure accurate flow measurement and control. Most importantly, for heats prone to slag inclusion, the standard argon flow rate was systematically reviewed and reduced based on real-time observation of mold level stability.

The results of this parameter adjustment are summarized in the table below. The “argon equivalent” is a normalized metric representing the total argon injection rate. A significant reduction of 27.8% was achieved post-improvement.

Table 2: Comparison of SEN Argon Injection Before and After Improvement
Period Avg. Argon Equivalent Change
Before Improvement (Jul-Dec 2019) 2.20 Baseline
After Improvement (Jan-Jun 2020) 1.59 -27.8%

Lower, stable argon flow directly contributed to a calmer meniscus and reduced the driving force for slag entrainment, thereby diminishing the frequency of slag inclusion defects.

3. Strict Control of Mold Level Fluctuation

A dedicated campaign was launched to minimize mold level fluctuation. This involved stabilizing the level measurement system against interference, optimizing PID control parameters in the automatic level control system, and changing the mold powder feeding practice from an automatic adjustment to a fixed feeding line strategy to ensure consistent thermal conditions. The improvement was tracked using a “Level Fluctuation Qualification Index,” where a higher score indicates better stability.

Table 3: Trend of Mold Level Fluctuation Qualification Index (Jan-Jun 2020)
Month Qualification Index
January 5.05
February 6.50
March 5.87
April 7.80
May 8.25
June 9.33

The index showed a clear upward trend, with an overall improvement of approximately 85% by June, confirming much tighter control over the meniscus and a corresponding reduction in conditions favorable for slag inclusion formation.

4. Implementation of Constant Speed Casting

For automotive steel grades, a strict constant speed casting practice was enforced. Standards for casting speed vs. slab section and steel throughput were defined and adhered to. Logistics were synchronized to minimize disruptions necessitating speed changes. The magnitude of any required speed adjustment was also limited. This practice promotes stable fluid flow patterns, aids inclusion floatation, and prevents transient surges that cause slag entrainment.

The percentage of cast length produced within the strict constant speed window showed marked improvement over the six-month period.

Table 4: Improvement in Constant Casting Speed Rate (Jan-Jun 2020)
Month Constant Speed Rate (%)
January 82.83
February 85.30
March 86.10
April 89.30
May 94.51
June 93.18

5. Supporting Measures

Additional supporting measures included stringent control of tundish superheat within the specified range, regular laser-guided checks and correction of SEN alignment, and careful sequencing of heats to avoid extremely low tundish weights during grade changes, which can disturb flow and temperature stability.

Results and Economic Impact

The synergistic implementation of these countermeasures yielded significant and measurable results in reducing slag inclusion defects.

The most direct internal metric, the slab blockage rate at the rolling mill due to slag inclusion defects, showed a consistent downward trend. This reduction directly saved costs associated with slab grinding (scarifying), manual repair, and logistics delays caused by offline processing.

Table 5: Reduction in Rolling Mill Slag Inclusion Blockage Rate (Jan-Jun 2020)
Month Blockage Rate Due to Slag Inclusion (%)
January 6.3
February 5.8
March 5.1
April 4.5
May 4.0
June 3.6

Externally, the effectiveness was reflected in customer feedback. Complaints related to slag inclusion defects from automotive users decreased by approximately 50%. The direct financial losses incurred from customer claims and concessions due to these defects fell by an estimated 70% per month. The improvement in consistent, high-quality supply enhanced customer satisfaction and strengthened our position as a reliable supplier of premium automotive steel.

Conclusions

The systematic investigation and control of slag inclusion defects in automotive steel led to the following key conclusions:

  1. The stability of the meniscus during continuous casting is the single most critical factor in preventing the formation of slag inclusion defects. Any practice that promotes meniscus turbulence increases the risk of slag entrainment.
  2. Reducing argon injection flow to the minimum necessary to prevent nozzle clogging and rigorously implementing constant speed casting are two highly effective operational measures to achieve meniscus stability and thereby minimize slag inclusion defects.
  3. Enhancing steel cleanliness to reduce the population of endogenous inclusions (like alumina) helps stabilize the casting process by reducing the tendency for nozzle clogging, which is a root cause of subsequent disruptive corrective actions that promote slag inclusion.
  4. A holistic approach, addressing mold flux properties, fluid flow control via argon and casting speed, and process stability via level control, is required for sustainable improvement. Isolated measures are less effective.
  5. The significant reduction in slag inclusion defects translates directly into substantial economic benefits through lower internal rework and processing costs, reduced yield loss, and decreased external customer claims. This demonstrates that quality improvement initiatives targeting specific defect modes like slag inclusion are not only technically sound but also economically justified, delivering a strong return on investment by enhancing operational efficiency and customer trust.

The control of slag inclusion remains a dynamic challenge, requiring continuous monitoring and refinement of practices as casting conditions and product mix evolve. However, the principles established—prioritizing stability, understanding root causes, and implementing integrated countermeasures—provide a robust framework for ongoing quality excellence in automotive steel production.

Scroll to Top