In this research, I investigated the feasibility of reinforcing ductile iron crankshafts with continuous carbon fibers, focusing on the casting method and the interfacial behavior between the fiber and the iron matrix. The motivation arose from the fact that ductile iron crankshafts frequently fail under high tensile stress, and conventional strengthening methods such as alloying and heat treatment have reached their practical limits. My approach involved electroplating nickel onto the carbon fiber surface, embedding the treated fibers into sand molds, and then casting ductile iron around them. I systematically analyzed the tensile properties, microstructural features, and element distribution at the fiber–matrix interface. Throughout the experiments, I paid particular attention to sand casting defects such as porosity, poor wetting, and fiber agglomeration, which are critical for the success of the composite.
Carbon fibers possess outstanding specific strength and modulus, low density, and excellent high-temperature stability in inert atmospheres. However, their poor wettability with liquid iron and the tendency to form brittle interfacial compounds have limited their application in ferrous matrix composites. To address these challenges, I selected a nickel coating as a transition layer. Nickel not only improves the wettability between carbon fiber and iron but also acts as a diffusion barrier, preventing the direct contact of carbon with iron at elevated temperatures. In addition, nickel is beneficial to the spheroidization of graphite in ductile iron, as it can enhance the nodule count and matrix properties.
The entire experimental process encompassed three major parts: surface metallization of carbon fibers, sand mold casting with embedded continuous fibers, and comprehensive characterization of the resulting composites. I also conducted theoretical analysis of the oxidation behavior of carbon fibers during high-temperature casting, since sand casting defects are often aggravated by gas evolution and oxidation at the interface.
1. Surface Metallization of Carbon Fibers
The T700 carbon fibers used in this study had a tensile strength of 4.9 GPa, a modulus of 230 GPa, an elongation of 2.1%, and a density of 1.8 g/cm³. The average diameter of a single filament was 7 μm. The fibers were provided in the form of 6K tows (6000 filaments). Before electroplating, the fibers had to be cleaned of the surface sizing that is applied during manufacturing. I selected a high-temperature removal method using a heat treatment furnace. The temperature was set to 400°C, and the fibers were held at this temperature for 5 minutes. This process effectively volatilized the organic sizing without causing significant oxidation or degradation of the fiber properties. After de-sizing, the fibers became fluffy and slightly roughened, as confirmed by scanning electron microscopy (SEM). The removal of the sizing layer was a crucial step because any residual polymer would weaken the adhesion of the nickel coating and lead to sand casting defects such as interfacial debonding.
Next, the fibers were subjected to a chemical roughening treatment to increase the surface area and improve the mechanical keying between the fiber and the nickel deposit. I used a mixed strong acid solution of H₂SO₄ and HNO₃ in a volume ratio of 3:7. To avoid dangerous splashing, I first cooled the mixing vessel in an ice bath at 5°C, then gradually added the acids while stirring for 30 minutes. After that, the solution was allowed to warm to 35°C for the actual roughening process. The optimal roughening time was found to be 80 minutes. Under these conditions, the fibers exhibited uniformly distributed pits and micro-grooves of moderate size, as shown in SEM micrographs. If the roughening time was less than 80 minutes, the etched sites were too sparse to provide good adhesion; if it exceeded 100 minutes, the pits coalesced into large defects and the fiber surface began to peel off, degrading the mechanical properties. Therefore, I set the coarsening parameters to 30–40°C for 80 minutes.
The electroplating bath composition was as follows: nickel sulfate (NiSO₄) 225 g/L, nickel chloride (NiCl₂) 65 g/L, sodium chloride (NaCl) 55 g/L, boric acid (H₃BO₄) 40 g/L, and sodium lauryl sulfate (C₁₂H₂₅SO₄Na) 0.05 g/L. The pH value was kept between 3 and 4.5, and the bath temperature was maintained at 25°C. I performed a series of plating experiments by varying the current density from 0.1 to 0.5 A/dm² and the deposition time from 2 to 10 minutes. After plating, the fiber tows were rinsed with deionized water and dried. The thickness of the nickel coating was evaluated from cross-sectional SEM images. The results indicated that the coating thickness increased linearly with both plating time and current density. For the purpose of this study, I aimed for a coating thickness of approximately 0.3 μm, which provided a smooth and dense nickel layer without forming dendritic structures. When the coating exceeded 0.5 μm, the surface became rough and nodular, leading to poor coating compactness.
Figure 1. Nickel-coated carbon fibers (macro view). The black fibers turned silver after electroplating, confirming a complete Ni layer.

The microstructural evolution of the nickel coating can be described in stages. Initially, nickel atoms nucleated preferentially at the active sites and grooves on the fiber surface, forming isolated islands. With increasing deposition time, these islands grew and coalesced until they covered the entire fiber surface. Beyond a certain thickness, the growth became non-uniform due to the inherent roughness of the fiber, and dendritic protrusions appeared. These dendrites are undesirable because they reduce the interfacial strength and increase the tendency for stress concentration. Therefore, I selected a plating time of 8 minutes at a current density of 0.5 A/dm², yielding a coating thickness of 0.3 μm that was both compact and uniform. The nickel coating adhered well to the carbon fiber due to the mechanical interlocking provided by the roughening treatment and the chemical affinity between nickel and the surface functional groups introduced during acid oxidation.
| Current density (A/dm²) | Time (min) | Thickness (μm) | Quality |
|---|---|---|---|
| 0.1 | 8 | 0.10 | Incomplete coverage |
| 0.2 | 8 | 0.18 | Uneven |
| 0.3 | 8 | 0.25 | Good |
| 0.4 | 8 | 0.28 | Good |
| 0.5 | 8 | 0.30 | Ideal |
| 0.5 | 10 | 0.52 | Dendritic, rough |
2. Sand Mold Casting and Fiber Embedding
In order to assess the composite under tensile loading, I designed a Y-shaped test block from which standard round tensile specimens could be machined. The dimensions of the Y-block sand mold are shown in a schematic drawing; the metal pattern was placed in a 400×250×200 mm sand box. The sand was a traditional clay-bonded silica sand with sufficient permeability, strength, refractoriness, and collapsibility. I manually rammed the sand in layers, each layer approximately 5 cm thick. During ramming, I used the small end of the tamper first, then the flat end to ensure uniform compaction. It was important not to ram too hard near the pattern to avoid damaging the cavity, but the central part had to be rammed slightly harder to resist the erosion of liquid iron.
A crucial part of the process was the embedding of the continuous carbon fiber tows. The tows were braided into a three-dimensional structure to improve their handling and mechanical anchoring. I tested two methods: (a) pre-embedding the fibers during sand preparation, and (b) fixing the fibers after the mold was completed using steel pins. The first method proved much more effective. Before ramming the sand, the fiber braid was placed across the mold cavity and clamped at both ends of the sand box so that it stayed taut. This prevented the fibers from being displaced by the high-density molten iron during pouring. The fibers were positioned at the lower part of the Y-block, which corresponds to the gauge section of the tensile specimens after machining. This positioning allowed the fibers to run exactly along the axis of the test bar, maximizing the reinforcing effect.
For the second method, after the mold was fully prepared, steel pins were inserted into the cavity to hold the fibers in place. However, because the fibers are light and the molten iron is heavy and hot, the pins softened and the fibers shifted during pouring. This led to misalignment and inevitable sand casting defects such as fiber bending, segregation, and even direct exposure of fibers to the metal stream. Therefore, I adopted the pre-embedding method throughout the main experiments.
Before pouring, I inserted a venting rod to create numerous small vent holes, which are essential for the escape of hot gases and for avoiding blowholes—one of the most common sand casting defects. A pouring cup was formed on the top of the mold with an angle of about 60°, and its walls were smoothed to ensure a laminar flow of the molten metal. The pouring basin also served to trap slag and impurities. The mold was then closed, and the cavity was protected by introducing argon gas for 10 minutes prior to pouring. This created a partially inert atmosphere, which was aimed at reducing the oxidation of carbon fibers during the pouring operation. Despite these precautions, complete oxygen exclusion was impossible in an open sand mold, so some oxidation of the fibers still occurred.
The ductile iron was melted in an induction furnace. The base iron composition is listed below. After spheroidization with a rare-earth magnesium alloy and inoculation with silicon-based inoculants, the iron was poured at approximately 1350°C. The pouring speed was controlled manually to ensure a steady fill without turbulence. After pouring, a layer of exothermic sand was placed on top of the mold to slow the cooling rate, which further reduced the risk of thermal stresses and hot tears. The mold was allowed to cool for about 4 hours before shakeout.
| Element | C | Si | Mn | S | P | Mg | RE | Cr | Cu | Sn |
|---|---|---|---|---|---|---|---|---|---|---|
| Base iron | 3.6–4.0 | — | 0.3–0.5 | 0.008–0.025 | ≤0.05 | — | — | ≤0.08 | — | — |
| After spheroidization | 3.5–3.8 | 1.8–2.0 | 0.3–0.5 | 0.008–0.025 | ≤0.05 | 0.035–0.055 | 0.006–0.03 | ≤0.08 | 0.2–0.3 | 0.015–0.025 |
After solidification, the Y-block was sectioned to remove the upper part, which contained more impurities and shrinkage porosity. The lower part was machined by CNC into round tensile specimens with a gauge diameter of 10 mm and a gauge length of 50 mm. Before machining, the location of the carbon fibers was identified using ultrasonic or visual inspection and marked. This precaution prevented accidental cutting of the fibers during machining. Eight specimens were fabricated: three contained uncoated carbon fibers (designated 1#, 2#, 3#) and five contained nickel-coated fibers (designated 4# to 8#).
3. Tensile Testing and Analysis of Sand Casting Defects
Tensile tests were performed using an MTS Exceed E45 electronic universal testing machine. The crosshead speed was set to 12.70 mm/min, and the initial gauge length was 50 mm. The fracture surfaces of the specimens were examined visually and under SEM. The tensile strength results are summarized in Table 3. The average tensile strength of the uncoated fiber specimens was 437 MPa, while that of the nickel-coated fiber specimens was 535 MPa, which is an improvement of 98 MPa. This significant increase can be attributed to the better interfacial bonding and the absence of massive voids in the nickel-coated fiber composite. In contrast, the uncoated fibers exhibited poor wetting with liquid iron, leading to large interfacial gaps and voids. These voids acted as stress concentrators and initiated premature cracks, resulting in lower tensile strength. The uncoated fibers were literally pulled out of the matrix when the specimen fractured, whereas the nickel-coated fibers broke together with the matrix, indicating effective load transfer across the interface.
| Specimen | Fiber type | Tensile strength (MPa) |
|---|---|---|
| 1# | Uncoated | 432 |
| 2# | Uncoated | 441 |
| 3# | Uncoated | 438 |
| 4# | Nickel-coated | 542 |
| 5# | Nickel-coated | 531 |
| 6# | Nickel-coated | 538 |
| 7# | Nickel-coated | 529 |
| 8# | Nickel-coated | 535 |
The presence of sand casting defects was more pronounced in the uncoated fiber specimens. The SEM images showed that the fiber tows remained as agglomerated bundles with no infiltration of iron between the individual filaments. The gap between the fibers and the matrix was significant, and the fiber surfaces were smooth and clean, indicating that the molten iron did not wet them. In the nickel-coated specimens, the fibers were uniformly distributed, and the iron matrix showed excellent infiltration between the filaments. The nickel layer dissolved partially in the iron, creating a metallurgical bond. This observation confirmed that the nickel coating effectively mitigated the poor wettability and prevented the formation of large-scale voids.
To further quantify the effect of nickel coating, I calculated the so-called “composite strengthening efficiency” using the rule of mixtures. The theoretical tensile strength of the composite, assuming perfect bonding and aligned continuous fibers, can be expressed as:
$$ \sigma_c = \sigma_f V_f + \sigma_m (1 – V_f) $$
where \(\sigma_c\) is the composite strength, \(\sigma_f\) is the fiber tensile strength, \(V_f\) is the fiber volume fraction, and \(\sigma_m\) is the matrix strength. In practice, the actual strength is always lower due to defects and imperfect interfaces. The difference between the theoretical and experimental values indicates the impact of sand casting defects and oxidation. For the uncoated fiber specimens, the experimental strength was much lower than the theoretical prediction, while for the nickel-coated specimens the gap was smaller, confirming that the coating reduced the severity of defects.
During the tensile tests, I also measured the elongation at break. The nickel-coated fiber specimens showed slightly lower elongation but higher ultimate tensile strength, suggesting a more brittle failure mode, which is typical for well-bonded composites. The uncoated fiber specimens exhibited a sawtooth-like stress–strain curve due to the successive pull-out and fracture of fibers, which is a clear indication of weak interfaces and internal delamination.
4. High-Temperature Oxidation of Carbon Fibers and Its Relation to Sand Casting Defects
Carbon fibers are known to be stable in inert atmospheres up to very high temperatures, but they oxidize rapidly in air above 400°C. In the presence of oxygen, the following reactions occur:
$$ C_{(s)} + O_2 \rightarrow CO_2_{(g)} $$
$$ 2C_{(s)} + O_2 \rightarrow 2CO_{(g)} $$
$$ 2CO + O_2 \rightarrow 2CO_2 $$
$$ C_{(s)} + CO_2 \rightarrow 2CO $$
At temperatures above 700°C, carbon dioxide itself acts as an oxidizing agent. The CO₂ molecules generated in the first two reactions diffuse to the fiber surface and react with carbon atoms, producing CO. This CO then diffuses outward and reacts with incoming oxygen to form CO₂, which again diffuses back to the fiber surface. This cyclic process consumes carbon atoms rapidly, leading to a significant reduction in fiber strength and an increase in surface porosity. The oxidized fibers become brittle and lose their load-bearing capacity. Such oxidation not only reduces the intrinsic fiber strength but also creates a gas film around the fiber, which prevents intimate contact between the fiber and the molten iron. This gas film is a primary cause of sand casting defects such as microbubbles and interfacial delamination in the final casting.
To model the oxidation process, I treated the fibers as right circular cylinders and considered the kinetics of the gas–solid reaction. In the kinetically controlled regime, the oxidation rate can be expressed in terms of the molar change of carbon:
$$ -\frac{dn}{dt} = k A c $$
where \(n = \frac{W}{M}\) is the number of moles of carbon, \(W\) is the weight of the fiber, \(M\) is the molar mass of carbon, \(A\) is the surface area, \(c\) is the oxygen concentration at the fiber surface, and \(k\) is the reaction rate constant. The negative sign indicates the loss of mass. For a cylindrical fiber of radius \(r\) and length \(l\), the surface area is \(A = 2 \pi r l\), and the molar amount of carbon is \(n = \pi r^2 l \rho/M\), where \(\rho\) is the fiber density. Substituting and simplifying gives the rate of radius change:
$$ \frac{dr}{dt} = – \frac{k c}{\rho} $$
Integrating from the initial radius \(r_0\) to \(r=0\) yields the time for complete burn-off:
$$ t_{ox} = \frac{\rho r_0}{k c} $$
This equation shows that the oxidation time is directly proportional to the initial fiber radius and inversely proportional to the oxygen concentration. In other words, increasing the fiber diameter or reducing the oxygen concentration both prolong the oxidation time. In the present casting process, the oxygen concentration is not zero even with argon purging, so some oxidation inevitably occurs. However, the nickel coating can act as a partial barrier, reducing the direct exposure of carbon to the oxidizing environment. The SEM/EDS analysis of fibers after casting revealed that uncoated fibers had a much higher oxygen content than nickel-coated fibers. For uncoated fibers, the EDS spectrum showed 68.65% carbon, 21.10% oxygen, and some iron (6.43%), indicating the formation of iron oxides or iron carbides at the interface. In contrast, nickel-coated fibers contained 78.65% carbon, 7.77% oxygen, and 2.21% nickel, with almost no iron. This confirms that the nickel layer suppressed the interfacial reaction between carbon and iron, thus avoiding the formation of brittle Fe₃C, which is harmful to the ductility and toughness of the composite.
To avoid oxidation completely, the following strategies are recommended: (a) vacuum casting, where the partial pressure of oxygen is extremely low; (b) casting in a fully sealed chamber with argon or another inert gas; or (c) applying an impermeable ceramic coating that isolates the fiber from the atmosphere during pouring. The last option is easier to implement in conventional sand foundries, but it adds an additional process step. The oxidation model presented above provides a useful framework for estimating the acceptable oxygen concentration or the required fiber radius to maintain fiber integrity during the cooling period.
5. Interfacial Microstructure and Bonding Mechanisms
The interface is the heart of any composite material. In this study, the interface between carbon fiber and ductile iron determines the overall mechanical performance. I investigated the interfacial morphology using optical microscopy and scanning electron microscopy, and analyzed the elemental distribution using energy-dispersive X-ray spectroscopy (EDS). The specimens were cut from the gauge section of the tensile bars using a wire-cutting machine, then ground with SiC papers from 400 to 2000 grit, and polished with diamond paste. Extreme care was taken during polishing to minimize the washing away of small particles and to retain the true interfacial features.
Optical microscopy at different magnifications showed a dramatic contrast between the coated and uncoated fibers. In the uncoated fiber composites, the fibers appeared as dark agglomerates, and the iron matrix was separated from the fiber bundles by large gaps. These gaps are classic sand casting defects caused by poor wetting and solidification shrinkage. At 100× magnification, individual fibers were clearly visible, but they were not surrounded by iron; instead, the iron had formed a wall around the fiber bundle, leaving a hollow channel. This morphology is a direct confirmation of non-wetting. In the nickel-coated fiber composites, the matrix was in intimate contact with the fibers at all magnifications. At 10× magnification, the fibers were well distributed and embedded in the iron matrix without visible defects. At 50× and 100× magnification, the interface appeared continuous, and the matrix had infiltrated the spaces between the filaments, indicating that the nickel coating had promoted wetting.
Scanning electron microscopy of the fracture surfaces provided further evidence. Figure 6 (a,b,c) showed uncoated fibers: (a) a low-magnification cross-section revealing a large elongated void where fibers had been pulled out; (b) a higher-magnification view showing clean fiber surfaces with no iron attached; (c) a close-up showing the fiber–matrix gap. In contrast, Figure 6 (d,e,f) displayed nickel-coated fibers: (d) a low-magnification view of the fracture surface with no macro voids; (e) a higher-magnification image showing iron clinging to the fiber surfaces; (f) a close-up of a single coated fiber embedded in the matrix, confirming the excellent bonding.
The EDS mapping of the uncoated fiber fracture surface demonstrated that carbon was confined to the fiber bundle and iron was absent in that region, proving that liquid iron did not penetrate the bundle. This lack of infiltration is one of the most severe sand casting defects in fiber-reinforced metals, and it directly leads to premature failure under load. In the nickel-coated specimens, EDS mapping showed a uniform distribution of carbon, iron, and nickel. Importantly, nickel was not restricted to the fiber surface; it had diffused into the iron matrix, creating a gradient zone. This diffusion was driven by the concentration difference between the high-nickel layer and the iron matrix. The formation of a Fe-Ni solid solution at the interface promotes strong metallurgical bonding, and the remains of the nickel layer on the fiber side form a carbide-like product that also enhances adhesion.
To quantify the element gradients, I performed point analysis at three locations across the interface: (a) in the iron matrix away from the fiber, (b) at the interfacial region, and (c) in the center of the fiber. The results are summarized in Table 4. At point (a), the iron content was highest (greater than 95 wt%), while carbon and nickel were low. At point (b), the iron content was still about 70 wt%, but nickel had increased to about 15 wt%, and carbon was about 10 wt%. At point (c), carbon was the dominant element (greater than 85 wt%), with small amounts of nickel and iron. This data confirms that the nickel coating acted as a diffusion source, creating a transition zone of several micrometers in thickness. The presence of nickel in the iron matrix near the interface is beneficial because it improves the toughness and strength of the matrix in that local region, and it also reduces the driving force for crack propagation along the interface.
| Point | C | Fe | Ni | Other |
|---|---|---|---|---|
| Matrix away from fiber | 2.5 | 96.1 | 0.2 | 1.2 |
| Interface region | 12.3 | 72.4 | 13.8 | 1.5 |
| Center of fiber | 86.5 | 1.2 | 8.9 | 3.4 |
The reaction between nickel and carbon at high temperature can form nickel carbide (Ni₃C), although this phase is not always stable at room temperature. The presence of Ni₃C at the interface may contribute to a chemical bond between the nickel layer and the carbon fiber. Meanwhile, the nickel layer on the outer side dissolves into the iron matrix, forming a Fe-Ni solid solution. The overall interface can be characterized as a Fe-Ni-C gradient structure, with metallurgical bonding from the iron to the nickel to the carbon fiber. This type of interface is beneficial because it transfers the load by atomic bonding rather than by mechanical interlocking, which is usually weak. The reduction of sand casting defects in terms of voids and gaps was directly observed from SEM images. No such gaps were found in the nickel-coated composites.
6. The Role of Sand Casting Defects on Composite Performance
Throughout the study, I repeatedly observed that sand casting defects were the primary cause of property degradation in the uncoated fiber composites. Defects appeared in several forms: (1) macro-voids caused by fiber agglomeration and poor infiltration; (2) micro-porosity resulting from gas evolution during fiber oxidation; (3) interfacial gaps formed by differential thermal contraction; and (4) brittle reaction products such as Fe₃C that form at the interface. The nickel coating effectively mitigated all these defects except for the intrinsic oxidation that occurs in the thin boundary layer around fibers. Even with argon purging, the sand mold cannot be made fully impermeable to air, so some oxygen is always present. However, the nickel layer substantially reduced the extent of oxidation, as evidenced by the lower oxygen content in the EDS spectra.
I also noticed that the pre-embedding method of fiber placement was instrumental in avoiding another type of sand casting defects—namely fiber misalignment and fiber washout. When fibers are placed in the mold cavity after ramming, the force of the liquid metal can easily displace them, leading to a non-uniform distribution and even exposure of fibers to the outer surface. Pre-embedding the fibers and keeping them tensioned during ramming ensures that they remain exactly in the desired position. This is particularly important for continuous fiber reinforcement, because even a small deviation from the load direction dramatically reduces the strengthening efficiency.
During the pouring process, the turbulent flow of molten iron can entrap gases and create bubbles. These bubbles become fixed during solidification, resulting in blowholes. The use of a proper pouring cup, vent holes, and the controlled pouring speed reduces turbulence. In my experiments, I poured the iron steadily and ensured that the mold cavity was completely filled before the metal began to solidify. The argon purging before pouring also helped to replace some of the air in the cavity, further reducing the risk of gas-related defects.
7. Conclusions and Outlook
In this work, I successfully demonstrated a method to incorporate continuous carbon fibers into ductile iron using sand mold casting, with nickel-coated fibers providing significantly better performance than uncoated fibers. The main conclusions are as follows:
1. The electroplating of nickel on T700 carbon fibers can be optimized using a bath with pH 3–4.5 at 25°C, a current density of 0.5 A/dm², and a deposition time of 8 minutes, leading to a uniform 0.3 μm-thick nickel layer. Roughening of the fiber surface in a 3:7 H₂SO₄/HNO₃ solution at 35°C for 80 minutes is essential to ensure good adhesion of the nickel layer.
2. Pre-embedding the carbon fiber braid in the sand mold before ramming keeps the fibers taut and correctly positioned. This avoids fiber displacement and reduces sand casting defects related to agglomeration and misalignment. Purging the mold cavity with argon for 10 minutes before pouring helps to suppress oxidation, although complete inertization is not possible in an open sand mold.
3. The tensile strength of ductile iron specimens containing nickel-coated carbon fibers was 535 MPa, which is 98 MPa higher than those containing uncoated fibers (437 MPa). The improvement is attributed to better interfacial wetting and the elimination of large voids. The nickel-coated fibers fractured simultaneously with the matrix, indicating effective load transfer.
4. High-temperature oxidation of carbon fibers occurs when the temperature exceeds 700°C, consuming carbon atoms and producing CO/CO₂. This oxidation not only degrades the fiber itself but also causes gas evolution, leading to sand casting defects such as microbubbles and interfacial porosity. To avoid oxidation, casting should be performed in a vacuum or in a fully inert atmosphere. Alternatively, a ceramic coating can serve as an oxygen barrier.
5. The nickel coating improved the interfacial wettability and bonding. EDS analysis revealed that nickel diffused from the coating into the iron matrix, creating a concentration gradient and forming a Fe-Ni solid solution near the interface. The remaining nickel at the fiber side reacted with carbon to form Ni₃C, enhancing adhesion. Consequently, the interface can be described as a Fe-Ni-C metallurgical bond, which is far superior to the mechanical contact existing in uncoated fiber composites.
6. The presence of brittle Fe₃C at the interface of uncoated fiber specimens was detected, which is harmful to the mechanical properties. In nickel-coated specimens, no Fe₃C was observed, confirming that the nickel layer acts as a diffusion barrier preventing the direct contact between carbon and iron.
Looking forward, there are several promising avenues to further improve the composite properties. First, the use of advanced fiber architectures, such as three-dimensional woven preforms, can create a continuous network of reinforcement and eliminate the weak planes that exist in unidirectional composites. Second, the optimization of the nickel coating thickness and the introduction of multilayered coatings (e.g., Ni + TiC or Ni + Y₂O₃) could provide better oxidation resistance and interfacial control. Third, the application of external pressure during solidification, such as squeeze casting, could suppress the remaining sand casting defects and improve fiber infiltration. Fourth, the development of a vacuum-assisted sand casting process would minimize oxidation and gas entrapment, further increasing the reliability of the composite.
In conclusion, the combination of nickel electroplating and sand mold casting with pre-embedded continuous carbon fibers provides a practical route to enhance the tensile strength of ductile iron crankshafts. The results of this research not only clarify the interfacial behavior of the Fe-C system with a nickel intermediate layer but also provide quantitative data for future casting process simulation. By carefully controlling the surface treatment of fibers, the mold design, and the pouring parameters, the negative effects of sand casting defects can be minimized, and the full potential of carbon fiber reinforced ductile iron can be realized. This approach may eventually lead to the production of lighter, stronger, and more durable crankshafts for automotive and industrial applications.