Introduction
As modern industries such as marine engineering, vehicle manufacturing, aerospace, and aviation increasingly demand lightweight materials, cast aluminum alloys have gained prominence due to their excellent corrosion resistance and superior castability. These alloys can rapidly produce components with complex geometries through sand casting processes. However, during the solidification process, coarse microstructures often develop, leading to various sand casting defects such as shrinkage porosity, segregation, hot tearing, and gas porosity. These sand casting defects significantly deteriorate mechanical properties including strength, ductility, and toughness. Therefore, refining the solidification structure of cast aluminum alloys represents a critical approach to enhancing mechanical performance and minimizing sand casting defects.
The pouring process constitutes a critical step in casting formation, with the pouring cup serving as an essential component of the gating system. In my research, I have redesigned the pouring cup to enable pulsed magnetic field treatment of molten metal. Based on factory sand casting pouring procedures, I conducted laboratory simulations using a pulsed magnetic field generator to investigate its effects on the solidification structure and mechanical properties of ZL205A alloy, thereby establishing an experimental foundation for pouring cup design.
Utilizing COMSOL Multiphysics software, I developed multi-physics coupling models for two types of pouring cups, achieving visualization of magnetic field, flow field, and temperature field distributions within the melt. My comparative analysis examined how different pouring cup structures and electromagnetic parameters influence these distributions. The simulation results demonstrated that the plug-type pouring cup with inner coil differential loading, operating at 20 Hz, 50% duty cycle, and 200 A, could process a melt volume of 4.37×10⁷ mm³ with dB/dt reaching 10480 mT/s. The small-type pouring cup achieved a magnetic field processing volume of 6.28×10⁶ mm³ with dB/dt reaching 8960 mT/s.
I subsequently constructed pouring platforms for both cup designs and experimentally verified that ZL205A and ZL114A aluminum alloy melts treated with pulsed magnetic fields within the pouring cups exhibited refined grain structures and enhanced mechanical properties, confirming the feasibility of these designs.

Cast Aluminum Alloys and Sand Casting Defects
Cast aluminum alloys are classified into several systems based on primary alloying elements: Al-Si, Al-Cu, Al-Mg, and Al-Zn. The Al-Si system accounts for 80% to 90% of all aluminum castings due to its excellent casting properties, low shrinkage rate, and good corrosion resistance. Al-Cu alloys exhibit outstanding mechanical properties at elevated temperatures with simple melting and casting processes. Al-Mg alloys combine low density with high strength and superior corrosion resistance. Al-Zn alloys demonstrate high strength even in as-cast conditions.
ZL205A Aluminum Alloy
ZL205A belongs to the Al-Cu-Mn system and represents one of the highest-strength cast aluminum alloys globally. Table 1 presents its chemical composition. The alloy achieves its exceptional properties through a combination of strengthening mechanisms: Cu forms Al₂Cu precipitates uniformly dispersed in the matrix during heat treatment; Mn forms T-phase to enhance mechanical properties; Ti and Zr form intermetallic compounds with Al that promote fine equiaxed grain formation; and B and Cd contribute to microstructural refinement.
Table 1: Chemical composition of ZL205A alloy (wt%)
| Element | Cu | Mn | Ti | Zr | B | V | Cd | Al |
|———|—–|—–|—–|—–|—–|—–|—–|—–|
| Content | 4.6–5.3 | 0.3–0.5 | 0.15–0.35 | 0.05–0.2 | 0.005–0.06 | 0.05–0.3 | 0.15–0.25 | Bal. |
ZL114A Aluminum Alloy
ZL114A belongs to the Al-Si-Mg system and exhibits excellent castability, low thermal expansion coefficient, and good corrosion resistance. Table 2 shows its chemical composition. The alloy contains 6.5–7.5% Si, which forms eutectic structures that enhance fluidity and reduce hot tearing tendency, while Mg contributes through Mg₂Si phase formation. Ti acts as a grain refiner, and Be forms a dense oxide film that protects the melt from oxidation.
Table 2: Chemical composition of ZL114A alloy (wt%)
| Element | Si | Mg | Ti | Be | Fe | Cu | Al |
|———|—–|—–|—–|—–|—–|—–|—–|
| Content | 6.5–7.5 | 0.45–0.75 | 0.08–0.25 | ≤0.07 | ≤0.2 | ≤0.1 | Bal. |
Laboratory Simulation of Sand Casting Process
Based on traditional sand casting procedures, I conducted laboratory experiments to simulate the pouring process and investigate pulsed magnetic field effects on ZL205A alloy. The experimental setup included an induction coil, resistance furnace, crucible, and preheated graphite molds. The process involved heating the alloy to 730 °C, applying pulsed magnetic field treatment for 90 seconds, and pouring at 700 °C into molds preheated to 300 °C.
Table 3 summarizes the experimental electromagnetic parameters:
Table 3: Electromagnetic parameters for laboratory experiments
| No. | Frequency (Hz) | Duty Cycle (%) | Peak Current (A) | dB/dt (mT/s) |
|—–|—————-|—————-|——————|————–|
| 1 | 0 | 0 | 0 | 0 |
| 2 | 20 | 20 | 100 | 3150 |
| 3 | 40 | 20 | 100 | 8000 |
| 4 | 50 | 20 | 100 | 150000 |
Effect on Primary α-Al Phase
My metallographic examination revealed that without pulsed magnetic field treatment, the solidification structure consisted primarily of coarse, irregularly shaped rosette crystals with low sphericity and poor distribution uniformity. Application of pulsed magnetic field treatment significantly refined these structures. At dB/dt of 3150 mT/s, the rosette crystals became finer with increased numbers of small, rounded grains. Further increasing dB/dt to 8000 mT/s produced optimal refinement, transforming most coarse rosette crystals into uniformly distributed, spheroidal microparticles. However, at 15000 mT/s, some coarse rosette crystals reappeared.
Table 4 presents the quantitative grain size measurements:
Table 4: Average α-Al grain size under different dB/dt values
| dB/dt (mT/s) | Edge Grain Size (μm) | Center Grain Size (μm) |
|————–|———————-|———————-|
| 0 | 71.53 | 80.45 |
| 3150 | 61.31 | 69.67 |
| 8000 | 52.34 | 62.46 |
| 15000 | 61.59 | 70.67 |
Effect on Al₂Cu Phase Morphology
Scanning electron microscopy analysis revealed that Al₂Cu phase existed as coarse network structures in untreated samples. After applying pulsed magnetic field at 8000 mT/s, the Al₂Cu phase transformed dramatically. The edge regions exhibited fine, fragmented structures, while the center regions showed fragmentation into small, nearly spherical particles. This morphological evolution from continuous networks to discrete particles indicates that pulsed magnetic field effectively refines both primary α-Al and Al₂Cu phases.
Effect on Mechanical Properties
The mechanical properties showed significant improvement after pulsed magnetic field treatment. Table 5 summarizes the tensile test results:
Table 5: Mechanical properties of ZL205A alloy under different dB/dt
| dB/dt (mT/s) | Yield Strength (MPa) | Tensile Strength (MPa) | Elongation (%) |
|————–|———————|————————|—————-|
| 0 | 125 | 206 | 6.0 |
| 3150 | 145 | 225 | 8.5 |
| 8000 | 160 | 241 | 11.5 |
| 15000 | 140 | 218 | 7.5 |
At the optimal dB/dt of 8000 mT/s, yield strength increased by 28%, tensile strength by 17.5%, and elongation by 91.66%. Hardness measurements showed increases of 13% at the edge and 9.3% at the center. Fracture surface analysis revealed that untreated samples exhibited shallow, sparse dimples, while treated samples showed numerous deep dimples, indicating improved ductility.
Mechanism of Grain Refinement
The grain refinement mechanism under pulsed magnetic fields can be understood through thermodynamics. The critical activation energy for nucleation with magnetic energy is expressed as:
$$\Delta G_m^* = \frac{16\pi\sigma_{sl}^3}{3\left[\Delta G_v + \mu_0\Delta\chi_{L-S}|H|^2/2\right]^2} \tag{1}$$
where μ₀ is vacuum permeability, ΔχS-L is the change in volume magnetic susceptibility between solid and liquid phases, H is magnetic field intensity, and ΔGv is the Gibbs free energy difference between liquid and solid phases.
The nucleation rate per unit volume per unit time is given by:
$$I = n_s^*\varepsilon v n e^{-\Delta G_m^* / kT} e^{-Q/kT} \tag{2}$$
where k is Boltzmann’s constant, Q is diffusion activation energy, ns* is the number of atoms on a critical nucleus surface, ε is the probability of atomic jumping in a given direction, and v is the vibrational frequency of liquid atoms.
When pulsed magnetic field is applied, the melt absorbs electromagnetic energy, which provides additional driving force for nucleation, thereby reducing the energy barrier for formation of critical nuclei. This leads to increased nucleation rates and consequently finer grain structures. According to the Hall-Petch relationship:
$$\sigma_b = \sigma_0 + kd^{-1/2} \tag{3}$$
where σb is tensile strength, d is average grain size, k is a material constant, and σ₀ is lattice resistance to unit dislocation movement. The refined grain size directly contributes to enhanced mechanical properties.
Furthermore, the mean radius of atomic clusters in the melt can be described by:
$$R(T) = r\left[\alpha Z_1^2 \left(\frac{1+C_0}{C_0}\exp\left(\frac{\Delta G_r^*}{k}\left(\frac{1}{T} – \frac{1}{T_m}\right)\right)\right)^{-1} – 1\right] \tag{4}$$
Pulsed magnetic field energy promotes the collision and combination of atomic clusters, facilitating the formation of crystal embryos. The repeated process of cluster formation and dissociation under the magnetic field homogenizes atomic distribution, leading to grain refinement.
Multi-Physics Mathematical Model of Pouring Cup
I employed COMSOL Multiphysics software to establish multi-physics coupling models for two pouring cup configurations. The models incorporate magnetic field, flow field, and temperature field interactions within the melt.
Model Assumptions and Simplifications
To simplify the complex physical phenomena while maintaining accuracy, I adopted the following assumptions:
1. The melts are considered incompressible Newtonian fluids with negligible density variations, with thermal buoyancy described by the Boussinesq approximation
2. No deformation of the melt occurs under magnetic force
3. Since the magnetic Reynolds number Rm << 1, the influence of flow field on electromagnetic field is negligible
4. Displacement currents are neglected due to the perfect conductivity of molten metals
5. Transverse heat conduction is negligible compared to normal heat flux
Governing Equations
The electromagnetic field is described by Maxwell’s equations. The magnetic flux density and current density distributions are governed by:
$$\nabla \times \vec{H} = \vec{J} + \frac{\partial \vec{D}}{\partial t} \tag{5}$$
$$\nabla \times \vec{E} = -\frac{\partial \vec{B}}{\partial t} \tag{6}$$
$$\nabla \cdot \vec{B} = 0 \tag{7}$$
The current density follows Ohm’s law:
$$\vec{J} = \sigma\vec{E} \tag{8}$$
The Lorentz force and electromagnetic heat generated are:
$$\vec{F} = \vec{J} \times \vec{B} \tag{9}$$
$$Q = \vec{J} \cdot \vec{E} \tag{10}$$
For the fluid flow and heat transfer, the conservation equations are employed. The mass conservation equation:
$$\frac{\partial \rho}{\partial t} + \nabla \cdot (\rho\vec{U}) = 0 \tag{11}$$
The momentum conservation equation:
$$\frac{\partial(\rho\vec{U})}{\partial t} + \nabla \cdot (\rho\vec{U}\vec{U}) = \nabla \cdot (\mu_{eff}\nabla\vec{U}) – \nabla P + S_m \tag{12}$$
The energy conservation equation:
$$\frac{\partial(\rho T)}{\partial t} + \nabla \cdot (\rho\vec{U}T) = \nabla \cdot \left(\frac{k}{c_p}\nabla T\right) + S_{th} \tag{13}$$
The momentum source term includes thermal buoyancy and time-averaged electromagnetic force:
$$S_m = F_m + S_i \tag{14}$$
$$S_i = \rho g\beta(T – T_0) \tag{15}$$
$$F_m = \frac{1}{T_p}\int_0^{T_p} f dt \tag{16}$$
For turbulence modeling, I adopted the standard k-ε model:
$$\frac{\partial(\rho k)}{\partial t} + \nabla \cdot (\rho\vec{U}k) = \nabla \cdot \left[\left(\mu + \frac{\mu_t}{\sigma_k}\right)\nabla k\right] + G_k – \rho\varepsilon + S_k \tag{17}$$
$$\frac{\partial(\rho\varepsilon)}{\partial t} + \nabla \cdot (\rho\vec{U}\varepsilon) = \nabla \cdot \left[\left(\mu + \frac{\mu_t}{\sigma_\varepsilon}\right)\nabla\varepsilon\right] + C_1\frac{\varepsilon}{k}G_k – C_2\rho\frac{\varepsilon^2}{k} + S_\varepsilon \tag{18}$$
The turbulent viscosity is expressed as:
$$\mu_t = \rho C_\mu\frac{k^2}{\varepsilon} \tag{19}$$
Table 6 lists the constants used in the k-ε model:
Table 6: Constants in the k-ε model
| Constant | C₁ | C₂ | σₖ | σε | Cμ |
|———-|—–|—–|——|——-|——|
| Value | 1.44 | 1.92 | 1.0 | 1.3 | 0.09 |
Material Properties and Boundary Conditions
Table 7 presents the magnetic properties of materials used in the simulation:
Table 7: Magnetic properties of materials
| Parameter | Melt | Air | Iron Core | Coil |
|———–|——|—–|———–|——|
| Relative permeability μ₀ | 1 | 1 | B-H curve | 1 |
| Relative permittivity ε₀ | 1 | 1 | 1 | 1 |
| Conductivity σ (S/m) | 3.71–8.77×10⁶ | 0 | 3.18×10⁷ | 1.72×10⁶ |
The boundary conditions included far-field magnetic insulation (B=0 at the outer boundary of air domain), static adiabatic walls for melt side and bottom surfaces, and free surface heat transfer at the melt top with a heat transfer coefficient of h=25 W/(m²·°C).
Numerical Simulation Results and Analysis
Comparison of Different Pouring Cup Structures
I designed and compared three configurations for the plug-type pouring cup: single-ended, inner-side, and symmetric coil arrangements. Table 8 compares their magnetic field treatment performance:
Table 8: Comparison of different pouring cup structures
| Structure | Treatment Volume (mm³) | Volume Fraction (%) | dB/dt (mT/s) |
|———–|————————|——————–|————–|
| Single-ended | 2.68×10⁷ | 17.87 | 10480 |
| Inner-side | 4.37×10⁷ | 29.13 | 10480 |
| Symmetric | 3.05×10⁷ | 20.33 | 10480 |
The inner-side configuration demonstrated superior performance by treating 29.13% of the total melt volume, meeting the requirement of ≥25% while maintaining the target dB/dt value.
Effect of Magnetic Field Direction
I investigated the influence of coil connection methods on magnetic field distribution. When coils were connected in the same direction (uniform magnetic field), the treatment volume was 3.13×10⁷ mm³, representing 20.89% of the total volume. In contrast, opposite-direction coil connections (differential magnetic field) generated a more vortex-like electromagnetic force distribution that enhanced melt flow and achieved a larger treatment volume of 4.37×10⁷ mm³ (29.13%). Therefore, I selected the differential field configuration for optimal performance.
Effects of Frequency and Duty Cycle
Parametric studies examined the influence of frequency (20-50 Hz) and duty cycle (20-50%) on magnetic field distribution. Table 9 summarizes the dB/dt values and treatment volumes:
Table 9: Effects of frequency and duty cycle on magnetic field parameters
| Frequency | Duty Cycle | dB/dt (mT/s) | Volume (mm³) |
|———–|————|————–|————–|
| 20 Hz | 20% | 8920 | 2.96×10⁷ |
| 20 Hz | 40% | 10100 | 3.89×10⁷ |
| 20 Hz | 50% | 10480 | 4.37×10⁷ |
| 40 Hz | 20% | 12600 | 2.31×10⁷ |
| 40 Hz | 40% | 13800 | 3.12×10⁷ |
| 40 Hz | 50% | 14200 | 3.45×10⁷ |
| 50 Hz | 20% | 14800 | 2.15×10⁷ |
| 50 Hz | 40% | 15600 | 2.78×10⁷ |
| 50 Hz | 50% | 16000 | 3.08×10⁷ |
My analysis revealed that lower frequencies combined with higher duty cycles achieve smaller dB/dt values within the target range of 8000-15000 mT/s while providing larger treatment volumes. The combination of 20 Hz and 50% duty cycle produced optimal results with dB/dt of 10480 mT/s and treatment volume of 4.37×10⁷ mm³.
The magnetic field attenuation in the melt exhibited exponential decay characteristics:
$$B(x) = B_0 e^{-\alpha x} \tag{20}$$
where B₀ is the surface magnetic flux density, α is the attenuation coefficient, and x is the distance from the surface. Higher frequencies resulted in faster attenuation due to increased skin effect, while higher duty cycles enabled deeper penetration.
Effect of Current Intensity
Table 10 presents the influence of current intensity on magnetic field parameters:
Table 10: Effect of current intensity on magnetic field parameters
| Current (A) | dB/dt (mT/s) | Volume Fraction of B>10mT (%) |
|————-|————–|——————————-|
| 100 | 5256 | 16.41 |
| 150 | 7888 | 23.77 |
| 200 | 10480 | 29.13 |
At 100 A, the Lorentz force caused melt to converge toward the coil center from both sides, with flow concentrated near the coil and a stagnation zone in the middle. Increasing to 200 A expanded the flow region, eliminated dead zones, and promoted stronger internal convection. The velocity at the monitoring point increased from 0.031 m/s to 0.049 m/s, representing a 58% enhancement.
The temperature field analysis showed that without magnetic field, heat accumulated at the horizontal center due to weak natural convection, creating significant temperature gradients. Applying pulsed magnetic field generated forced convection, which improved heat exchange between upper and lower melt regions, reduced temperature differences, and enhanced temperature uniformity throughout the melt.
Small Pouring Cup Simulation
For the small pouring cup design, the annular configuration achieved a dB/dt of 8960 mT/s, within the target range of 8000-15000 mT/s. The magnetic field exhibited a characteristic saddle-shaped distribution with higher intensity near the coil ends and lower intensity at the center. Importantly, the magnetic field exceeded 10 mT throughout the entire melt volume, ensuring sufficient treatment across the complete melt.
The flow field analysis revealed four vortices with maximum velocity of 0.05 m/s distributed in the outer annular region. The temperature field showed clear division into high-temperature and low-temperature zones, with the upper region experiencing more effective cooling due to electromagnetic force-induced convection.
Model Verification
I validated the numerical model against experimental measurements using Hall sensors and oscilloscopes. The actual current waveform was loaded into the numerical model, and the simulated magnetic flux density was compared with experimental data. The maximum peak magnetic field measured was 98 mT, while the simulated value was 92 mT, representing a difference of only 6.52%. This close agreement confirms the reliability and feasibility of the numerical model for engineering design purposes.
Manufacturing and Application of Pouring Cups
Plug-Type Pouring Cup
Based on the simulation results, I manufactured a plug-type pouring cup suitable for large sand castings. The cup dimensions were 834×700×590 mm with a maximum capacity of 1.6×10⁸ mm³. The structure adopted an I-shape with a funnel-shaped bottom to reduce impact during pouring. Key components included the pulsed magnetic field generator, pouring box, lifting rings, sockets, cooling fan, fixing frame, support frame, and sprue.
The magnetic field generator consisted of induction coils wound with 70 mm² cross-section wire around iron cores, totaling 120 turns. The iron cores measured 80×180×140 mm. The box was constructed from 304 stainless steel to avoid magnetic interference, with thermal insulation plates inside to protect the coils from excessive temperatures and maintain melt temperature.
For the field experiments, I selected ZL205A and ZL114A alloys. The experimental procedure involved heating the melt to 730 °C, sealing the sprue with a plug, pouring the melt into the pouring cup, and applying pulsed magnetic field treatment for 240 seconds. When the temperature dropped to 663 °C, a portion of the melt was extracted for test bar casting, and the plug was removed to allow the remaining melt to flow into the sand mold.
Table 11 summarizes the plug-type pouring cup experimental parameters:
Table 11: Plug-type pouring cup experimental parameters
| No. | dB/dt (mT/s) | Magnetizing Temp (°C) | Pouring Temp (°C) | Treatment Time (s) |
|—–|————–|———————–|——————-|———————|
| 1 | 0 | 730 | 663 | 240 |
| 2 | 10480 | 730 | 663 | 240 |
The experimental results demonstrated significant microstructural refinement. Without magnetic field treatment, the primary α-Al phase consisted of coarse rosette crystals with poor roundness. With dB/dt of 10480 mT/s, the α-Al grains transformed into smaller, more spheroidal particles. Quantitative analysis showed the average grain size decreased from 62.27 μm to 50.64 μm, representing 18.7% refinement.
Table 12 presents the mechanical properties of ZL205A as-cast test bars:
Table 12: Mechanical properties of ZL205A as-cast test bars
| dB/dt (mT/s) | Tensile Strength (MPa) | Elongation (%) | Hardness (HV) |
|————–|————————|—————-|—————-|
| 0 | 309 | 7.0 | 54 |
| 10480 | 349 | 12.5 | 70 |
The pulsed magnetic field treatment increased tensile strength by 12.9%, elongation by 78.6%, and hardness by 29.6%. Table 13 shows the T5 heat-treated mechanical properties of ZL205A castings:
Table 13: T5 heat-treated mechanical properties of ZL205A castings
| dB/dt (mT/s) | Tensile Strength (MPa) | Elongation (%) | Hardness (HBW) |
|————–|————————|—————-|—————-|
| 0 | 236 | 3.5 | 116 |
| 10480 | 350 | 10.0 | 125 |
After T5 heat treatment, the tensile strength increased by 48.31%, elongation by 185.71%, and hardness by 7.76%. Similarly, ZL114A castings exhibited improvements of 15.05% in tensile strength and 5.21% in hardness after pulsed magnetic field treatment, confirming the effectiveness of this approach in reducing sand casting defects and enhancing material performance.
Small Pouring Cup
I manufactured a small pouring cup designed for smaller sand molds. The device dimensions were φ404/260×222 mm, with coils wound from 4×8 mm single conductors in a ring configuration: 6 layers × 20 turns, totaling 120 turns with a height of 200 mm. The design incorporated 10 mm insulation felt to maintain temperatures below 100 °C and ventilation openings for coil cooling.
For this configuration, I performed experiments with ZL114A alloy using five different dB/dt values to optimize the treatment parameters. Table 14 summarizes the test bar experiment parameters:
Table 14: Small pouring cup test bar experiment parameters
| No. | dB/dt (mT/s) | Magnetizing Temp (°C) | Pouring Temp (°C) |
|—–|————–|———————–|——————-|
| 1 | 0 | 730 | 700 |
| 2 | 8960 | 730 | 700 |
| 3 | 17600 | 730 | 700 |
| 4 | 18400 | 730 | 700 |
| 5 | 23000 | 730 | 700 |
The as-cast microstructure examination revealed that all pulsed magnetic field treatments refined the primary α-Al phase compared to untreated samples. At low and high dB/dt values (8960 and 23000 mT/s), the structure consisted of fine equiaxed grains, while intermediate values (17600 and 18400 mT/s) produced less complete refinement with some dendritic morphology.
Table 15 presents the average grain size measurements:
Table 15: Average α-Al grain size of ZL114A alloy
| dB/dt (mT/s) | Grain Size (μm) | Refinement (%) |
|————–|—————–|—————-|
| 0 | 77.66 | – |
| 8960 | 60.89 | 21.59 |
| 17600 | 66.91 | 13.84 |
| 18400 | 65.31 | 15.91 |
| 23000 | 61.57 | 20.72 |
The mechanical property tests, summarized in Table 16, confirmed that the optimal dB/dt was 8960 mT/s, providing the best combination of strength and ductility:
Table 16: Mechanical properties of ZL114A as-cast test bars
| dB/dt (mT/s) | Tensile Strength (MPa) | Elongation (%) | Hardness (HV) |
|————–|————————|—————-|—————-|
| 0 | 199.75 | 5.12 | 68.44 |
| 8960 | 240.00 | 9.00 | 77.14 |
| 17600 | 215.00 | 6.50 | 72.50 |
| 18400 | 220.50 | 7.20 | 73.80 |
| 23000 | 232.00 | 8.50 | 75.90 |
Based on these results, I selected dB/dt values of 8960 and 23000 mT/s for sand mold casting experiments. Table 17 presents the T5 heat-treated mechanical properties of ZL114A castings:
Table 17: T5 heat-treated mechanical properties of ZL114A sand castings
| dB/dt (mT/s) | Tensile Strength (MPa) | Elongation (%) | Hardness (HV) |
|————–|————————|—————-|—————-|
| 0 | 200.00 | 6.52 | 67.16 |
| 8960 | 262.00 | 9.02 | 81.68 |
| 23000 | 254.50 | 7.55 | 78.56 |
At the optimal parameter of 8960 mT/s, the tensile strength increased by 31%, elongation by 38.34%, and hardness by 21.62% compared to untreated castings. These improvements demonstrate that applying pulsed magnetic field treatment in the pouring cup effectively refines the solidification structure and enhances mechanical properties, thereby mitigating the occurrence of sand casting defects.
Conclusions
Through systematic laboratory experiments, numerical simulations, and field applications, I have drawn the following conclusions:
1. Laboratory experiments on ZL205A alloy demonstrated that pulsed magnetic field treatment at dB/dt of 8000 mT/s optimally refines the solidification structure. The primary α-Al grain size decreased by up to 26.83%, while yield strength, tensile strength, and elongation increased by 28%, 17.5%, and 91.66% respectively. The hardness improvements were 13% at the edge and 9.3% at the center.
2. Numerical simulations established that the plug-type pouring cup should adopt the inner-side coil configuration with differential magnetic field direction, while the small pouring cup should use annular design. The optimal electromagnetic parameters of 20 Hz frequency, 50% duty cycle, and 200 A current provide the largest magnetic field treatment volume while maintaining dB/dt within the design range.
3. The plug-type pouring cup field experiments confirmed that pulsed magnetic field treatment effectively refines ZL205A alloy, with T5 heat-treated tensile strength increasing by 48.31% and elongation by 185.71%. The treatment also significantly reduced the presence of sand casting defects in the final components.
4. The small pouring cup experiments established that a dB/dt value of 8960 mT/s provides optimal treatment for ZL114A alloy. The tensile strength increased by 31%, elongation by 38.34%, and hardness by 21.62% after T5 heat treatment, confirming the feasibility of this miniaturized design.
The pulsed magnetic field mechanism involves reducing the activation energy for nucleation through electromagnetic energy absorption, which promotes atomic cluster formation and increases nucleation rates. The refined grain structure, governed by the Hall-Petch relationship, directly contributes to enhanced mechanical properties and reduced sand casting defects. These developed pouring cups provide an effective technical solution for improving cast aluminum alloy quality in industrial sand casting processes.