In this work, I focused on the sand casting process of a horizontal split pump body made of 00Cr25Ni6Mo2N duplex stainless steel. The harsh service environment, including corrosive media, high pressure, and complex flow conditions, imposes strict requirements on the mechanical properties, corrosion resistance, and structural integrity of the pump body. However, duplex stainless steel exhibits poor castability due to its wide solidification range, large solidification shrinkage, and susceptibility to hot cracking. Thus, the key challenge is to minimize sand casting defects such as shrinkage porosity, gas holes, and inclusions. Through numerical simulation, mixture design optimization, and process parameter tuning, I aimed to improve the casting quality and reduce the occurrence of these defects.
1. Introduction
Duplex stainless steels have been developed for nearly a century and are now widely used in petrochemical, marine, and nuclear industries because of their excellent combination of high strength and outstanding corrosion resistance. The two-phase microstructure, consisting of approximately equal amounts of austenite and ferrite, provides superior resistance to chloride stress corrosion cracking and pitting compared with conventional austenitic stainless steels. The material 00Cr25Ni6Mo2N belongs to the third-generation duplex stainless steel grade, with a nominal composition of 25–28% Cr, 4.5–6.5% Ni, 1.2–2.0% Mo, and 0.08–0.2% N. Although this grade exhibits excellent service performance, its casting characteristics are challenging. The wide solidification range leads to a pasty solidification mode, making the alloy prone to shrinkage porosity and hot tearing. Moreover, the high chromium content increases melt viscosity and oxidation tendency, causing oxide inclusions and cold shuts. These issues are typical sand casting defects that must be addressed through careful process design.
Several domestic and international studies have been conducted on duplex stainless steel castings. For example, some researchers used corundum sand and controlled heat treatment to reduce cracking in valve bodies. Others optimized the gating system and applied chills to produce large duplex stainless steel impellers. However, each casting component has its own unique structure and solidification characteristics, so a case-specific investigation is necessary.
In this study, I designed two sand casting process schemes for the pump body, constructed digital models using UG NX, and performed numerical simulations using AnyCasting software. The simulation results were used to compare the two schemes and select a better one. I then optimized the chemical composition of the alloy through a D-optimal mixture design, improved the feeding and cooling system, and optimized the pouring parameters. Additionally, I developed a simple and low-cost method for phase ratio analysis of duplex stainless steel using MATLAB image processing. The ultimate goal was to eliminate sand casting defects and guarantee the quality of the pump body casting.
2. Casting Process Design and Numerical Simulation
2.1 Pump Body and Material Properties
The pump body is a large complex casting with an overall length of 1660 mm, width of 1100 mm, and height of 850 mm. The rough casting weighs about 1400 kg. Its structure consists of a volute chamber, four flanges, four support legs, and a middle split surface with shaft bores. The wall thickness varies from 16 mm to 89 mm, creating significant thermal nodes. The flanges and split surface are functional surfaces that require high density and pressure tightness. During service, the pump body must withstand hydraulic pressure and corrosive media, so internal shrinkage defects are strictly limited. The chemical composition of the material is given in Table 1.
| Element | C | Si | Mn | P | S | Cr | Ni | Mo | N |
|---|---|---|---|---|---|---|---|---|---|
| Content | ≤0.05 | ≤1.00 | ≤2.00 | ≤0.035 | ≤0.030 | 25–28 | 4.5–6.5 | 1.2–2.0 | 0.08–0.2 |
Table 2 lists the required mechanical properties. The yield strength must exceed 550 MPa, and the tensile strength should be in the range 800–880 MPa. These requirements demand not only proper melting and heat treatment but also defect-free castings.
| Property | Tensile strength σb (MPa) | Yield strength σ0.2 (MPa) | Elongation δ (%) |
|---|---|---|---|
| Value | 800–880 | ≥550 | ≥20 |
2.2 Numerical Simulation Fundamentals
Numerical simulation is a powerful tool for predicting filling and solidification behavior and for identifying potential sand casting defects. The governing equations for melt flow include the continuity, momentum, and energy equations. For incompressible viscous flow, the continuity equation can be written as:
$$\frac{\partial \rho}{\partial t} + \frac{\partial (\rho u)}{\partial x} + \frac{\partial (\rho v)}{\partial y} + \frac{\partial (\rho w)}{\partial z} = 0$$
where \(u, v, w\) are the velocity components in the \(x, y, z\) directions, and \(\rho\) is the density. The momentum equation (Navier–Stokes) is:
$$\rho\left(\frac{\partial u}{\partial t} + u\frac{\partial u}{\partial x} + v\frac{\partial u}{\partial y} + w\frac{\partial u}{\partial z}\right) = -\frac{\partial p}{\partial x} + \rho g_x + \mu \nabla^2 u$$
$$\rho\left(\frac{\partial v}{\partial t} + u\frac{\partial v}{\partial x} + v\frac{\partial v}{\partial y} + w\frac{\partial v}{\partial z}\right) = -\frac{\partial p}{\partial y} + \rho g_y + \mu \nabla^2 v$$
$$\rho\left(\frac{\partial w}{\partial t} + u\frac{\partial w}{\partial x} + v\frac{\partial w}{\partial y} + w\frac{\partial w}{\partial z}\right) = -\frac{\partial p}{\partial z} + \rho g_z + \mu \nabla^2 w$$
The energy conservation equation is expressed as:
$$\rho C_p \frac{\partial T}{\partial t} = k\left(\frac{\partial^2 T}{\partial x^2} + \frac{\partial^2 T}{\partial y^2} + \frac{\partial^2 T}{\partial z^2}\right)$$
In the solidification simulation, the heat transfer includes conduction, convection, and radiation. The conduction equation with latent heat release is:
$$\rho C_p \frac{\partial T}{\partial t} = \frac{\partial}{\partial x}\left(\lambda \frac{\partial T}{\partial x}\right) + \frac{\partial}{\partial y}\left(\lambda \frac{\partial T}{\partial y}\right) + \frac{\partial}{\partial z}\left(\lambda \frac{\partial T}{\partial z}\right) + Q$$
where \(Q = \rho L \frac{\partial f_s}{\partial t}\) is the latent heat source term.
To predict shrinkage defects, I used the Niyama criterion and the residual melt modulus method. The Niyama criterion is defined as:
$$N = \frac{G}{\sqrt{R}}$$
where \(G\) is the temperature gradient and \(R\) is the cooling rate. A small \(N\) value indicates a high risk of micro-shrinkage. For macro-shrinkage, the residual melt modulus is:
$$M_r = \frac{V_r}{A_r}$$
where \(V_r\) is the volume of the isolated residual liquid and \(A_r\) is its surface area. A larger \(M_r\) indicates a greater tendency for shrinkage porosity.
2.3 Initial Process Schemes
Two sand casting process schemes were designed. Both used furan resin sand molds and cores, with chromite sand for the flow channel cores. The pouring system was designed with ceramic tubes to resist erosion. Scheme 1 placed the sprue on the parting line with a middle injection configuration. Scheme 2 used a step gating system at the inlet and outlet flanges. The pouring temperature was set to 1560°C and the initial mold temperature to 25°C. Figure 1 shows the simulation model used in this study.

I modeled the two schemes using UG NX and imported the STL files into AnyCasting. The mesh consisted of 1.5 million finite difference cells. Table 3 summarizes the simulation parameters for both schemes.
| Parameter | Scheme 1 | Scheme 2 |
|---|---|---|
| Number of cells | 1,500,000 | 1,500,000 |
| Process | Sand casting | Sand casting |
| Analysis type | Filling and solidification | Filling and solidification |
| Liquidus temperature | 1453°C | 1453°C |
| Solidus temperature | 1357°C | 1357°C |
| Shrinkage rate | 2% | 2% |
| Initial mold temperature | 25°C | 25°C |
| Pouring temperature | 1560°C | 1560°C |
| Gravity direction | -Z | -Z |
2.4 Comparison and Selection
The filling simulation showed that Scheme 1 took 28 seconds to fill, while Scheme 2 took 27 seconds. Scheme 1 exhibited turbulence at the beginning of filling due to the middle injection, causing sand erosion and possible oxide inclusions. Scheme 2 had some initial “turbulent” flow in the upper gate, but the overall filling was smoother. The temperature distribution at the end of filling was more uniform for Scheme 2. The solidification sequence was similar, but Scheme 2 had a slightly shorter solidification time (3401 s) than Scheme 1 (3505 s). Using the Niyama criterion and the residual melt modulus, I quantitatively compared the shrinkage defect probability. Tables 4 and 5 present the statistical results.
| Item | Scheme 1 | Scheme 2 |
|---|---|---|
| Total measured cells | 95,700 | 99,753 |
| Cells with probability > 0.9 | 262 | 267 |
| Percentage of defective cells | 0.2738% | 0.2677% |
| Item | Scheme 1 | Scheme 2 |
|---|---|---|
| Total measured cells | 95,700 | 99,753 |
| Cells with probability > 0.9 | 279 | 247 |
| Percentage of defective cells | 0.2915% | 0.2476% |
Scheme 2 showed a lower probability of sand casting defects, especially in the flange areas. Therefore, I selected Scheme 2 as the basis for further improvement. However, the simulation revealed that the feeding capability of the step gating system was insufficient for the thick flanges. In addition, the top gates caused some undesirable turbulence. These issues were addressed in the subsequent process improvement.
3. Chemical Composition Optimization Using D-Optimal Mixture Design
The chemical composition of the duplex stainless steel directly affects its mechanical properties and corrosion resistance. To ensure the pump body can withstand aggressive media and high pressure, I optimized the composition with respect to yield strength (σ0.2) and pitting resistance equivalent number (PREN). I employed a D-optimal mixture design because the composition is constrained by the alloy specification and the sum of all components must equal 100%. The nine alloying elements (C, Si, Mn, P, S, Cr, Ni, Mo, N) were treated as independent variables, while the balance was iron (Fe). The constraints are listed in Table 6.
| Factor | Minimum (%) | Maximum (%) |
|---|---|---|
| Carbon | 0.03 | 0.05 |
| Silicon | 0 | 1 |
| Manganese | 0 | 2 |
| Phosphorus | 0 | 0.035 |
| Sulfur | 0 | 0.03 |
| Chromium | 25 | 28 |
| Nickel | 4.5 | 6.5 |
| Molybdenum | 1.3 | 2 |
| Nitrogen | 0.05 | 0.2 |
The total of the nine factors was fixed at 37%. I assumed a full quadratic response model and generated 55 experimental runs using Design-Expert software. The responses, PREN and yield strength, were evaluated using JMatPro material modeling software to avoid costly and time-consuming physical experiments. For the yield strength, a grain size of 2 μm was used, corresponding to the actual microstructure observed in the castings. PREN was calculated directly from the empirical formula:
$$\text{PREN} = \%\text{Cr} + 3.3 \cdot \%\text{Mo} + 16 \cdot \%\text{N}$$
Although JMatPro provides a more refined calculation, the above formula was used as a reference. The regression models obtained from the mixture design are given below:
$$Y_{\text{PREN}} = -503.39A + 37.81B + 37.80C + 22.23D + 36.84E + 34.99F + 37.81G + 28.73H + 0.93J + \cdots$$
$$Y_{\sigma_{0.2}} = -15253.67A + 761.36B + 674.20C + 4647.83D – 3.419\times10^5 E + 599.4F + 788.42G + 866.44H + 2112.17J + \cdots$$
where the variables A, B, C, D, E, F, G, H, J correspond to C, Si, Mn, P, S, Cr, Ni, Mo, N, respectively. The full interaction terms were included but are omitted here for compactness. The analysis of variance showed that the models were highly significant with \(P < 0.0001\) and adjusted \(R^2\) values of 1.000 for PREN and 0.980 for yield strength, indicating excellent predictive capability.
Figure 2 shows the relative importance of individual factors obtained from the regression coefficients. It was evident that carbon, sulfur, and phosphorus had the strongest influence on the responses. In particular, sulfur severely reduced the yield strength, while carbon increased the pitting resistance equivalent but also increased the risk of carbide precipitation. Based on a multi-objective optimization with the goal of maximizing PREN while keeping yield strength above 700 MPa, the optimum composition was determined as shown in Table 7.
| Element | C | Si | Mn | P | S | Cr | Ni | Mo | N |
|---|---|---|---|---|---|---|---|---|---|
| Content (%) | 0.04 | 1.0 | 1.0 | 0.01 | 0.025 | 28.0 | 4.7 | 2.0 | 0.2 |
This composition was then used for the subsequent melting and pouring simulations. The modified composition increased the liquidus temperature to 1474°C and decreased the solidus temperature to 1333°C, which was taken into account in the updated simulation model.
3.1 Melting and Charge Calculation
To achieve the target composition, I calculated the furnace charge using a linear equation method based on mass conservation. The charge materials included return scrap, pure iron, low-carbon stainless steel scrap, ferrochromium, ferromanganese, nickel plates, molybdenum wire, ferrosilicon, and chromium nitride. The element absorption rates (\(R\)) were determined from industrial practice. The mass balance equations are:
$$\sum_i m_i e_{ij} = \frac{M w_e}{R} – m_{\text{return}} e_{\text{return},i}$$
$$\sum_i m_i = M$$
where \(m_i\) is the mass of a given charge material, \(e_{ij}\) is the elemental content in that charge, \(M\) is the total batch mass (500 kg), \(w_e\) is the target element content, and \(R\) is the absorption rate. The resulting matrix equation \(AX = B\) was solved in Excel. Table 8 shows the calculated charge masses for a 500 kg batch with 30% return scrap.
| Charge material | Mass (kg) |
|---|---|
| Return scrap | 150 |
| Pure iron | 1.75 |
| Low-carbon stainless steel scrap | 236.78 |
| Ferrochromium | 90.69 |
| Ferromanganese | 1.65 |
| Nickel plate | 6.43 |
| Molybdenum wire | 1.84 |
| Ferrosilicon | 2.55 |
| Chromium nitride | 8.30 |
The calculated phosphorus and sulfur contents were 0.0127% and 0.0244%, respectively, which met the specification. This charge formula was recommended for production.
4. Casting Process Improvement and Simulation Verification
Based on the preliminary simulation, the selected Scheme 2 still had some problems. The most critical issue was the lack of effective feeding at the inlet and outlet flanges, which were the thickest sections and thus the last to solidify. In addition, the upper gate of the step gating system caused undesirable turbulence at the beginning of filling. I improved the process from three aspects: feeding system, cooling system, and gating system.
4.1 Improvement of Risers and Padding
To enhance the feeding capacity, I added two waist-shaped risers at the inlet and outlet flanges (designated 6# and 7#) with dimensions 400×100×300 mm and 320×100×300 mm, respectively. Furthermore, the existing top risers 1#, 2#, and 3# were changed from conventional sand risers to insulated risers with a 40 mm thick ceramic fiber sleeve. Insulated risers keep the liquid metal hot for a longer time, improving the feeding distance and reducing shrinkage porosity.
4.2 Application of Chills
The simulation indicated that the lower-middle part of the casting, including the shaft bore flanges, support legs, and the junction between the volute and the suction pipe, contained hot spots that were far from the risers. To accelerate solidification in these regions and break the isolated liquid pools, I placed 24 steel chills at selected locations. The chills were designed with different shapes, including plate chills and conformal chills, with volumes ranging from 20×100×150 mm to 40×120×200 mm. These chills effectively increased the local cooling rate and promoted a more favorable solidification pattern.
4.3 Gating System Modification
To solve the upper gate turbulence, I changed the step gating system to a “counter-angle” step design. The upper gate was moved to align with risers 4# and 5#, increasing the height difference between the upper and lower gates from 560 mm to 700 mm. The upper gate cross-section was enlarged to Φ45 mm to reduce the flow velocity. I also introduced a reverse sprue with a diameter of Φ65 mm and a primary sprue of Φ50 mm. This configuration prevented the upper gate from opening prematurely and ensured a smooth, sequential filling from bottom to top.
4.4 Simulation Verification of the Improved Process
I updated the simulation model with the modified geometry and the new material properties. The updated density, thermal conductivity, and specific heat as functions of temperature are shown in Table 9.
| Temperature (°C) | Density (g/cm³) | Thermal conductivity (W/(m·K)) | Specific heat (J/(g·K)) |
|---|---|---|---|
| 200 | 7.62 | 40.83 | 0.58 |
| 400 | 7.56 | 25.75 | — |
| 600 | 7.54 | 20.65 | 0.92 |
| 800 | 7.48 | 21.88 | 0.66 |
| 1000 | 7.32 | 29.33 | 0.72 |
| 1200 | 7.23 | 31.76 | 0.77 |
| 1400 | 7.13 | 33.92 | — |
| 1600 | 6.86 | 32.46 | 0.83 |
The filling simulation confirmed that the upper gate turbulence was eliminated, and the filling pattern was smooth and even. The final temperature distribution showed a stronger tendency for directional solidification from bottom to top. The solidification sequence demonstrated that the risers remained liquid until the end, effectively feeding the shrinkages. The residual melt modulus probability Mr decreased significantly. The percentage of defective cells was reduced to 0.2386% based on the residual melt modulus criterion. The casting yield was calculated to be 60.8%, which is acceptable for a medium-sized stainless steel casting.
5. Pouring Process Parameter Optimization
Although the casting process was improved, the pouring parameters still needed to be optimized to minimize sand casting defects further. I used an orthogonal experimental design to study the influence of pouring temperature, pouring time, and mold temperature on shrinkage porosity. The residual melt modulus Mr was used as the response variable because a smaller value indicates fewer defects. The factors and levels are listed in Table 10.
| Level | A: Pouring temperature (°C) | B: Pouring time (s) | C: Mold temperature (°C) |
|---|---|---|---|
| 1 | 1520 | 20 | 15 |
| 2 | 1540 | 35 | 25 |
| 3 | 1560 | 50 | 35 |
| 4 | 1580 | 65 | 45 |
I adopted the \(L_{16}(4^5)\) orthogonal array, which could accommodate up to five factors but only three were used. The simulation results for the sixteen runs are summarized in Table 11.
| Run | A (°C) | B (s) | C (°C) | Empty 1 | Empty 2 | Mr (mm) |
|---|---|---|---|---|---|---|
| 1 | 1520 | 20 | 15 | 1 | 1 | 44.921 |
| 2 | 1520 | 35 | 25 | 2 | 2 | 44.520 |
| 3 | 1520 | 50 | 35 | 3 | 3 | 44.232 |
| 4 | 1520 | 65 | 45 | 4 | 4 | 44.122 |
| 5 | 1540 | 20 | 25 | 3 | 4 | 45.334 |
| 6 | 1540 | 35 | 15 | 4 | 3 | 44.931 |
| 7 | 1540 | 50 | 45 | 1 | 2 | 44.767 |
| 8 | 1540 | 65 | 35 | 2 | 1 | 44.800 |
| 9 | 1560 | 20 | 35 | 4 | 2 | 45.906 |
| 10 | 1560 | 35 | 45 | 3 | 1 | 45.480 |
| 11 | 1560 | 50 | 15 | 2 | 4 | 45.085 |
| 12 | 1560 | 65 | 25 | 1 | 3 | 45.232 |
| 13 | 1580 | 20 | 45 | 2 | 3 | 45.503 |
| 14 | 1580 | 35 | 35 | 1 | 4 | 44.643 |
| 15 | 1580 | 50 | 25 | 4 | 1 | 45.625 |
| 16 | 1580 | 65 | 15 | 3 | 2 | 45.453 |
I performed an analysis of variance (ANOVA) to evaluate the significance of each factor. Table 12 presents the ANOVA results.
| Source | df | SS | MS | F ratio | F critical (0.05) |
|---|---|---|---|---|---|
| Pouring temperature | 3 | 2.303 | 0.767 | 2.970 | 3.29 |
| Pouring time | 3 | 0.778 | 0.259 | 1.003 | |
| Mold temperature | 3 | 0.193 | 0.064 | 0.249 | |
| Error | 15 | 3.880 | 0.259 | — |
The range analysis shown in Table 13 indicates the order of importance: A (pouring temperature) > B (pouring time) > C (mold temperature). The optimal combination was A1, B4, C3, i.e., pouring temperature 1520°C, pouring time 65 s, and mold temperature 35°C.
| Level | A | B | C | Empty 1 | Empty 2 |
|---|---|---|---|---|---|
| k1 | 44.449 | 45.416 | 45.098 | 44.891 | 45.206 |
| k2 | 44.958 | 44.893 | 45.178 | 44.977 | 45.162 |
| k3 | 45.426 | 44.927 | 44.895 | 45.125 | 44.974 |
| k4 | 45.306 | 44.902 | 44.968 | 45.167 | 44.796 |
| R | 0.977 | 0.523 | 0.283 | 0.255 | 0.041 |
The confirmation run with A1B4C3 produced the minimum Mr value of 44.122 mm, which was the same as run 4. The influence of mold temperature was negligible, as its range was close to that of the empty column. These results provided a robust recommendation for production.
6. A Simple Method for Phase Ratio Analysis of Duplex Stainless Steel
In the production of duplex stainless steel castings, it is essential to verify the phase balance (ferrite/austenite ratio) because it directly affects mechanical properties and corrosion resistance. The enterprise originally used manual grid counting, which was time-consuming and inaccurate. I developed a simple and low-cost method based on digital image processing with MATLAB. The basic principle is the same as quantitative metallography: the two phases can be distinguished by their different etching responses. After etching with a ferric chloride-hydrochloric acid solution, the ferrite phase appears light and the austenite phase appears dark in the optical micrograph. The RGB image is converted to grayscale and then binarized using a threshold determined by Otsu’s method. The Otsu algorithm maximizes the inter-class variance \(g\), defined as:
$$g = w_0 (u_0 – u)^2 + w_1 (u_1 – u)^2$$
where \(w_0\) and \(u_0\) are the proportion and mean gray level of the austenite class, \(w_1\) and \(u_1\) are those of the ferrite class, and \(u\) is the total mean gray level. The threshold that maximizes \(g\) gives the best separation between the two phases.
After binarization, the area fraction of austenite was calculated by counting the number of black pixels divided by the total number of pixels. The ferrite fraction was the complement. This method was applied to a typical micrograph of the 00Cr25Ni6Mo2N casting. The calculated austenite fraction was approximately 39.2%, while a commercial image analyzer (JX2000) gave a value of 38%. The close agreement validated the proposed method. The MATLAB code used for this analysis is shown in Figure 3.
This method significantly improves the efficiency and accuracy of phase ratio analysis without the need for expensive image-analysis equipment. It also helps to monitor the microstructure and to control sand casting defects related to phase imbalance, such as hot cracking and reduced corrosion resistance.
7. Conclusions and Outlook
In this work, I investigated the sand casting process of a duplex stainless steel horizontal split pump body with the aim of minimizing sand casting defects and ensuring high quality. The main conclusions are as follows:
1) The step gating system demonstrated superior performance over the middle injection system in terms of smooth filling and beneficial temperature distribution. The addition of insulated risers, chills, and an optimized gating system effectively reduced shrinkage porosity in the thick sections. The final simulation showed that the percentage of defective cells was reduced to 0.2386%, satisfying the quality requirements.
2) The D-optimal mixture design proved to be an efficient method for optimizing the chemical composition. Regression models for PREN and yield strength were established with high accuracy. The optimal composition was determined to be 0.04% C, 1.0% Si, 1.0% Mn, 0.01% P, 0.025% S, 28.0% Cr, 4.7% Ni, 2.0% Mo, and 0.2% N, which provided a good balance between corrosion resistance and mechanical strength. The melting charge was calculated using a linear equation model, yielding practical results for production.
3) The orthogonal experiment revealed that the pouring temperature was the most significant factor affecting shrinkage porosity, followed by pouring time, while mold temperature had a negligible effect. The optimal pouring parameters were 1520°C pouring temperature, 65 s pouring time, and 35°C mold temperature.
4) A simple, low-cost phase ratio analysis method was developed using MATLAB image processing. This method provides rapid and accurate determination of ferrite and austenite fractions, which is valuable for quality control in duplex stainless steel casting.
For future work, I plan to investigate the combined use of an intermediate frequency furnace and a VOD (vacuum oxygen decarburization) refining furnace to achieve better control of carbon content and cleanliness. The heat treatment parameters, including solution treatment and aging temperatures, also need to be optimized for this specific grade. Furthermore, the energy-saving and emission-reduction aspects of the casting foundry should be studied to promote green manufacturing.