In my work on heavy-section ductile iron castings, the most difficult metallurgical defect I have had to control is chunky graphite, also described in our internal reports as fragmented graphite. The defect appeared in a thick hydraulic rear cover produced from a QT450-type ductile iron casting. The wall thickness ranged from about 40 mm to 120 mm, and the molding route combined green sand molding, resin-bonded sand cores, medium-frequency induction melting, cored-wire spheroidization, and air-preloaded static pressure molding. When I dissected the first production castings, I found black patches in the thermal center of the thick section. In severe cases, the chunky graphite area occupied more than 30% of the examined section. The microstructure did not meet the design requirement, and the supply risk became serious. Therefore, I organized a systematic analysis of the melting materials, spheroidization treatment, molding process, solidification behavior, and local thermal conditions of the ductile iron casting.

The baseline composition window for the hydraulic rear cover is shown in Table 1. The alloy was designed as a ferritic-pearlitic ductile iron casting with controlled copper and tin. The original process used a magnesium-silicon-iron cored wire containing rare earth elements. The rare earth addition was intended to improve spheroidization, neutralize tramp elements, and stabilize graphite nucleation. However, in the thick section, the same rare earth addition became one of the main factors associated with chunky graphite. The thin walls of the same ductile iron casting did not show this defect, which told me that the problem was not simply a global chemical composition error. It was a local solidification and segregation problem.
| Material | C (%) | Si (%) | Mn (%) | S (%) | Cu (%) | Sn (%) | Mg (%) | RE (%) |
|---|---|---|---|---|---|---|---|---|
| Original baseline | 3.6–3.9 | 2.0–2.5 | 0.3–0.6 | ≤0.03 | 0.4–1.0 | 0.04–0.10 | 0.020–0.050 | 0.010–0.040 |
| QT450 target | 3.6–3.9 | 2.0–2.5 | 0.3–0.6 | ≤0.03 | 0.4–1.0 | 0.04–0.10 | 0.020–0.050 | 0.010–0.040 |
| Thin-wall region | 3.7–3.9 | 2.1–2.5 | 0.3–0.6 | ≤0.03 | 0.4–1.0 | 0.04–0.10 | 0.020–0.050 | 0.010–0.040 |
| Thick-wall region | 3.6–3.9 | 2.0–2.5 | 0.3–0.6 | ≤0.03 | 0.4–1.0 | 0.04–0.10 | 0.020–0.050 | 0.010–0.040 |
The carbon equivalent of the ductile iron casting was evaluated from the standard relationship for cast iron. I used this equation as a first check before I moved to local thermal analysis.
$$CE = C + \frac{Si}{3} + \frac{P}{3}$$
For the thick-section ductile iron casting, the local cooling rate is much lower than that in the thin wall. I used Chvorinov’s rule to compare the solidification time of different regions. The rule is especially useful because the hydraulic rear cover has a large hot spot in the center and several riser-neck hot spots.
$$t_s = B\left(\frac{V}{A}\right)^n$$
Here, \(t_s\) is the local solidification time, \(V\) is the volume of the local section, \(A\) is the heat-transfer surface area, \(B\) is a mold constant, and \(n\) is a power exponent usually close to 2 for many sand castings. For the thick center of the ductile iron casting, \(V/A\) is large, so \(t_s\) increases sharply. This explains why the same alloy can produce acceptable graphite in the thin wall but chunky graphite in the thick center.
The metallographic examination was performed on the dissected section. The black-patch region and the surrounding normal region were compared. The black-patch region contained many chunky, compact, and branched graphite particles. The normal region contained nodular graphite with a much higher nodularity. I defined the chunky graphite area fraction as follows:
$$A_{CG} = \frac{\sum A_i}{A_{total}} \times 100\%$$
where \(A_i\) is the area of each chunky graphite colony and \(A_{total}\) is the total examined area. I also defined nodularity as the fraction of graphite particles that meet the nodular shape criterion:
$$N = \frac{N_{VI} + N_V}{N_{total}} \times 100\%$$
where \(N_{VI}\) and \(N_V\) are the counts of acceptable nodular graphite particles and \(N_{total}\) is the total graphite count. The defect condition and the reference condition are summarized in Table 2.
| Region | Macro appearance | Microstructure | Graphite morphology | Risk level |
|---|---|---|---|---|
| Thick center, black patch | Dark, segregated black area | Chunky graphite colonies | Fragmented, branched, compact | High |
| Thick center, normal zone | Uniform grey | Nodular graphite in matrix | Mostly spherical | Low |
| Riser neck | Local dark spot | Mixed chunky and nodular | Partially degenerated | Medium to high |
| Thin wall | No black patch | Fine nodular graphite | Spherical | Low |
| Mold surface region | No black patch | Small nodules | Spherical | Low |
The thermal field simulation of the ductile iron casting was performed with a commercial solidification model. The simulation showed that the thick central section, the riser neck, and the upper part of the riser solidified later than the surrounding walls. These regions formed thermal hot spots and shrinkage porosity. The local solidification time in the center was several times larger than that in the thin wall. The cooling rate in the center was very low, which promoted long-range diffusion, rare earth segregation, and graphite degeneration. Table 3 summarizes the comparative thermal behavior of the ductile iron casting.
| Region | Relative thickness | Relative solidification time | Cooling rate | Hot spot tendency | Chunky graphite tendency |
|---|---|---|---|---|---|
| Thin wall | Low | Short | High | Low | Low |
| Intermediate wall | Medium | Medium | Medium | Medium | Low to medium |
| Thick center | High | Very long | Very low | Very high | Very high |
| Riser neck | High | Long | Low | High | High |
| Riser top | Medium to high | Long | Low | High | Medium to high |
From a solidification standpoint, the liquid-to-solid transformation range of ductile iron is sensitive to residual magnesium and rare earth content. I expressed the effective freezing range as a function of alloying and treatment variables:
$$\Delta T_{L-S} = T_L – T_S$$
and, in a simplified linear form for my analysis,
$$\Delta T_{L-S} = \Delta T_{L-S,0} + k_{Mg} w_{Mg} + k_{RE} w_{RE} – k_{Sb} w_{Sb}$$
Here, \(w_{Mg}\), \(w_{RE}\), and \(w_{Sb}\) are the mass fractions of residual magnesium, rare earth elements, and antimony, respectively. The coefficients \(k_{Mg}\), \(k_{RE}\), and \(k_{Sb}\) are positive or negative sensitivity factors determined from process data and literature trends. In my interpretation, a larger freezing range in the thick-section ductile iron casting extends the time during which carbon can diffuse away from the graphite interface. This favors chunky graphite instead of compact nodules.
The so-called section effect is central to the problem. In a thick-section ductile iron casting, the latent heat released during eutectic solidification is removed slowly. The local temperature remains high for a long time. The concentration and energy fluctuations needed for repeated nucleation are reduced. The number of active graphite nuclei decreases. At the same time, the austenite shell around the graphite can remain open for a long period. Carbon atoms can grow along the open liquid channels, leading to branched and chunky graphite. The defect is therefore not a simple shortage of magnesium. It is a combination of low cooling rate, long solidification time, rare earth grain-boundary segregation, and insufficient nodule nucleation.
I paid special attention to cerium and lanthanum because they are common rare earth elements in magnesium-silicon-iron cored wire. Ce and La tend to segregate to austenite grain boundaries. Their grain-boundary concentration can be described in a simplified segregation form:
$$C_{RE}^{GB} = C_{RE}^{0}\exp\left(-\frac{\Delta G_{RE}}{RT}\right)$$
where \(C_{RE}^{GB}\) is the grain-boundary concentration, \(C_{RE}^{0}\) is the bulk concentration, \(\Delta G_{RE}\) is the segregation free energy, \(R\) is the gas constant, and \(T\) is temperature. When Ce and La accumulate at austenite grain boundaries, the austenite surrounding the graphite may remain unclosed for a longer time. Carbon can then diffuse along the remaining liquid channels, and the graphite shape becomes irregular. This is one of the most important mechanisms I identified in the thick-section ductile iron casting.
I also reviewed the role of antimony. Sb is a strong grain-boundary segregating element. It can compete with rare earth elements for grain-boundary sites and modify interfacial energy and carbon activity. In some heavy-section ductile iron castings, a very small antimony addition can refine graphite and suppress chunky graphite. However, the addition window is narrow. Too little Sb may not balance the rare earth effect. Too much Sb can promote undesirable pearlite or other carbides. Therefore, I treated Sb as a balancing element rather than a simple alloying addition. The balance parameter I used was
$$\Pi_{RE-Sb} = \frac{w_{Sb}}{w_{RE}}$$
with the target window determined experimentally. The initial hypothesis was that a controlled antimony addition would reduce the effective rare earth segregation at austenite grain boundaries, increase the number of graphite nodules, and stabilize nodular growth in the thick-section ductile iron casting.
| Element | Main role in ductile iron casting | Behavior in thick section | Effect on chunky graphite |
|---|---|---|---|
| Mg | Spheroidizing element | Residual Mg increases freezing range | Excess residual Mg can increase risk |
| Ce | Rare earth spheroidizer and tramp element neutralizer | Segregates to austenite grain boundaries | Promotes chunky graphite when unbalanced |
| La | Rare earth spheroidizer and tramp element neutralizer | Segregates to austenite grain boundaries | Promotes chunky graphite when unbalanced |
| Sb | Surface-active grain-boundary modifier | Segregates to boundaries and interfaces | Can balance rare earth effect and reduce chunky graphite |
| C | Graphite-forming element | Long diffusion distance in hot spot | Carbon transport causes branched growth |
| Si | Graphitizer and matrix strengthener | Promotes ferrite and graphite nucleation | Moderate increase can improve nodule count |
Based on this mechanism, I designed a three-level trial. The original process used a magnesium-silicon-iron cored wire with rare earth. The first trial used a magnesium-silicon-iron cored wire without rare earth. The second trial used the same rare earth-free cored wire and added antimony metal to the pouring ladle. The antimony addition was set at 0.015% by mass. The trial plan is shown in Table 4.
| Trial | Spheroidizing wire | Rare earth content | Sb addition | Expected effect |
|---|---|---|---|---|
| Original process | MgSiFe cored wire with RE | Present | None | Baseline; black patch expected |
| Trial 1 | MgSiFe cored wire without RE | Reduced | None | Partial reduction possible |
| Trial 2 | MgSiFe cored wire without RE | Reduced | 0.015% Sb | Balanced RE effect; no black patch expected |
The melting and treatment procedure was kept as constant as possible. I used medium-frequency induction melting, controlled charging, and a covered pouring ladle. The cored wire was fed at a controlled speed. The magnesium content in the wire was about 10%. In the antimony trial, I added a measured amount of antimony metal to the ladle before pouring. The process parameters are summarized in Table 5.
| Parameter | Original process | Trial 1 | Trial 2 |
|---|---|---|---|
| Base iron melting | Induction furnace | Induction furnace | Induction furnace |
| Spheroidizing method | Cored wire | Cored wire | Cored wire |
| Wire Mg content | 10% | 10% | 10% |
| Wire rare earth | Contained RE | No RE | No RE |
| Sb addition | 0 | 0 | 0.015% |
| Inoculation | Standard | Standard | Standard |
| Pouring temperature | Controlled | Controlled | Controlled |
| Molding line | Static pressure | Static pressure | Static pressure |
After casting, I dissected the hydraulic rear cover and examined the thick section. The results are shown in Table 6. The original process produced black patches with chunky graphite. Trial 1, which only removed rare earth from the cored wire, still produced black patches. This was a critical result. It told me that simply reducing rare earth content was not enough. The local solidification condition of the thick-section ductile iron casting remained unfavorable. Trial 2, which combined rare earth reduction with 0.015% Sb, produced no black patches. The graphite was nodular and well distributed. The result confirmed that the rare earth effect had to be balanced rather than merely reduced.
| Trial | Black patch | Chunky graphite area | Graphite shape | Nodularity trend | Acceptance |
|---|---|---|---|---|---|
| Original | Present | High, sometimes over 30% | Fragmented and branched | Low | Not accepted |
| Trial 1 | Present | Still high locally | Partly chunky | Low to medium | Not accepted |
| Trial 2 | Absent | Very low to none | Nodular and compact | High | Accepted |
I then compared the microstructure more quantitatively. The nodularity, nodule count, chunky graphite fraction, and maximum graphite size were measured at the same location in each trial. The improvements are listed in Table 7. The antimony-containing trial showed a significant increase in nodule count and nodularity, and a sharp decrease in chunky graphite area.
| Metric | Original process | Trial 1 | Trial 2 | Direction of improvement |
|---|---|---|---|---|
| Chunky graphite area fraction | High | Medium to high | Very low | Decrease |
| Nodularity | Low | Low to medium | High | Increase |
| Nodule count | Low | Low to medium | High | Increase |
| Graphite degeneracy | Severe | Moderate | Minor | Decrease |
| Black patch in thick center | Yes | Yes | No | Eliminated |
| Thin-wall graphite | Acceptable | Acceptable | Acceptable | Maintained |
The mechanism of antimony can be further understood through its competition with rare earth elements at grain boundaries. I used a simplified competitive segregation equation:
$$\theta_{Sb} = \frac{K_{Sb}w_{Sb}}{1 + K_{Sb}w_{Sb} + K_{RE}w_{RE}}$$
where \(\theta_{Sb}\) is the fractional occupation of grain-boundary sites by Sb, \(K_{Sb}\) and \(K_{RE}\) are adsorption coefficients for Sb and rare earth elements, and \(w_{Sb}\) and \(w_{RE}\) are bulk mass fractions. When Sb occupies a fraction of the austenite grain boundaries, the effective rare earth segregation is reduced. This delays the formation of rare earth-rich boundary films and allows the austenite shell to close more uniformly around the graphite. As a result, carbon diffusion becomes more symmetric, and the graphite remains nodular instead of becoming chunky.
I also considered the effect of antimony on graphite nucleation. A small amount of Sb can increase the number of active nucleation sites by modifying the interfacial energy between graphite and liquid. The nucleation rate can be expressed in a simplified form as
$$I = I_0 \exp\left(-\frac{\Delta G^*}{kT}\right)$$
where \(I\) is the nucleation rate, \(I_0\) is a kinetic pre-factor, \(\Delta G^*\) is the activation energy for nucleation, \(k\) is Boltzmann’s constant, and \(T\) is absolute temperature. If Sb lowers the effective activation barrier for graphite nucleation or increases the available nucleation sites, the nodule count increases. A higher nodule count reduces the diffusion distance for carbon and suppresses the growth of isolated chunky graphite colonies. This is consistent with the trial 2 results in the thick-section ductile iron casting.
The balance between rare earth and antimony was not the only variable. I also evaluated the role of residual magnesium, inoculation practice, pouring temperature, and mold temperature. The process window is summarized in Table 8. The key conclusion is that the antimony addition must be controlled together with residual magnesium, rare earth content, and local cooling conditions.
| Variable | Low condition | Target condition | High condition | Effect on chunky graphite |
|---|---|---|---|---|
| Residual Mg | Insufficient spheroidization | Controlled range | Excess freezing range | High Mg increases risk |
| Rare earth | Too low for neutralization | Low and controlled | Grain-boundary segregation | High RE increases risk |
| Sb | No balancing effect | 0.015% in trial | Excess pearlite or carbides | Balanced Sb reduces risk |
| Pouring temperature | Cold shuts and misruns | Controlled superheat | Longer solidification time | High superheat increases risk |
| Inoculation | Low nodule count | Strong and late inoculation | Fading or over-inoculation | Good inoculation reduces risk |
| Mold cooling | Slow cooling | Balanced cooling | Too fast for thick section | Slow cooling increases risk |
For production control, I translated the trial findings into a final composition and process window. The rare earth content in the cored wire was reduced or eliminated. The residual rare earth in the ductile iron casting was kept as low as practicable. Antimony was added at a controlled level near 0.015%. The carbon equivalent was maintained in the range suitable for QT450. The final process window is listed in Table 9.
| Parameter | Final target | Control method | Reason |
|---|---|---|---|
| C | 3.6–3.9% | Charge calculation and thermal analysis | Maintain eutectic graphite growth |
| Si | 2.0–2.5% | Charge and inoculation control | Promote graphite and ferrite |
| Mn | 0.3–0.6% | Charge control | Balance matrix strength |
| S | ≤0.03% | Desulfurization and charge control | Avoid spheroidization consumption |
| Cu | 0.4–1.0% | Charge and alloy addition | Control matrix and hardenability |
| Sn | 0.04–0.10% | Charge and alloy addition | Control pearlite without excess segregation |
| Mg | 0.020–0.050% | Cored-wire feed and thermal analysis | Ensure spheroidization without excess freezing range |
| RE | Low and controlled | Use rare-earth-free or low-RE wire | Reduce Ce and La grain-boundary segregation |
| Sb | About 0.015% | Ladle addition | Balance rare earth and refine graphite |
I also developed a statistical model to describe the chunky graphite response. The model treated the chunky graphite area fraction as a function of rare earth, antimony, residual magnesium, local solidification time, and inoculation intensity. A linearized form is
$$Y = \beta_0 + \beta_1 w_{RE} + \beta_2 w_{Sb} + \beta_3 w_{Mg} + \beta_4 t_s + \beta_5 I_{inoc} + \varepsilon$$
where \(Y\) is the chunky graphite area fraction or a transformed defect score, \(\beta_i\) are regression coefficients, \(t_s\) is local solidification time, \(I_{inoc}\) is inoculation intensity, and \(\varepsilon\) is residual error. The sign of \(\beta_1\) is expected to be positive because rare earth segregation promotes chunky graphite. The sign of \(\beta_2\) is expected to be negative in the controlled window because antimony balances the rare earth effect. The sign of \(\beta_4\) is expected to be positive because a longer solidification time increases the risk. The coefficient signs and practical meaning are summarized in Table 10.
| Variable | Symbol | Expected coefficient sign | Practical interpretation |
|---|---|---|---|
| Rare earth | \(w_{RE}\) | Positive | More Ce and La increase grain-boundary segregation |
| Antimony | \(w_{Sb}\) | Negative in controlled window | Sb balances RE and reduces chunky graphite |
| Residual Mg | \(w_{Mg}\) | Positive | Excess Mg widens freezing range |
| Solidification time | \(t_s\) | Positive | Longer time increases diffusion and degeneration |
| Inoculation intensity | \(I_{inoc}\) | Negative | More nuclei reduce chunky graphite |
The production implementation was carried out in several batches. I evaluated the rejection rate before and after the process change. The original process had a high rejection rate because of black patches and chunky graphite. Trial 1 did not solve the problem. Trial 2 reduced the rejection rate to a very low level. The production comparison is shown in Table 11. The improvement was achieved without changing the basic molding line or the casting geometry. The key change was the combination of rare earth control and antimony addition.
| Production stage | Chunky graphite rejection | Black patch frequency | Nodularity compliance | Overall quality |
|---|---|---|---|---|
| Original process | High | Frequent | Poor in thick section | Unstable |
| Trial 1 | Still high | Frequent | Poor to marginal | Not acceptable |
| Trial 2 | Low | Rare | Good | Acceptable |
| Optimized production | Very low | Very rare | Good | Stable |
I also used process capability indices to confirm stability. For nodularity, I defined
$$C_p = \frac{USL – LSL}{6\sigma}$$
and
$$C_{pk} = \min\left(\frac{USL – \mu}{3\sigma}, \frac{\mu – LSL}{3\sigma}\right)$$
where \(USL\) and \(LSL\) are the upper and lower specification limits, \(\mu\) is the process mean, and \(\sigma\) is the process standard deviation. After the process change, the nodularity of the thick-section ductile iron casting moved closer to the target and the variation decreased. This was especially important because the defect had previously appeared only in the thick section, while the thin section remained acceptable. A global average would have hidden the local problem. Therefore, I recommended that the quality control plan sample the thick hot spot separately from the thin wall.
From a practical standpoint, the antimony addition must be introduced carefully. I used a measured addition to the pouring ladle. The dissolution and recovery of Sb depend on ladle temperature, holding time, and stirring. A simple recovery expression is
$$\eta_{Sb} = \frac{w_{Sb,final} – w_{Sb,initial}}{w_{Sb,added}}$$
where \(\eta_{Sb}\) is the recovery ratio. In my trials, the target final Sb content was about 0.015%. If the recovery is low, the balance against rare earth is insufficient. If the recovery is too high, the risk of carbides or excessive pearlite increases. Therefore, I controlled the addition by weight and verified it by spectroscopy. The rare earth content was also monitored because the balance parameter \(\Pi_{RE-Sb}\) is sensitive to small changes in rare earth.
The thermal condition of the ductile iron casting also matters. I could not completely eliminate the thick-section hot spot because the hydraulic rear cover requires a thick central section for functional reasons. However, I could improve the local cooling by optimizing the riser position, chill placement, and mold material. The thermal simulation indicated that a modest increase in local cooling rate reduces the solidification time and the diffusion distance for carbon. The relationship can be written as
$$A_{CG} \propto \frac{1}{\dot{T}^m}$$
where \(A_{CG}\) is the chunky graphite area fraction, \(\dot{T}\) is the local cooling rate, and \(m\) is a positive exponent. This means that higher cooling rate tends to reduce chunky graphite. However, the cooling rate cannot be increased without limit because it may cause shrinkage porosity, hard edges, or residual stress. The final process therefore combined chemical balance with thermal balance.
I also examined the influence of inoculation. In a thick-section ductile iron casting, inoculation fades with time. Late inoculation is important because it provides nuclei when the melt reaches the eutectic stage. I used a late inoculation step and monitored the nodule count. The relationship between nodule count and chunky graphite can be expressed qualitatively as
$$A_{CG} \propto \frac{1}{N_n^q}$$
where \(N_n\) is the nodule count and \(q\) is a positive exponent. A higher nodule count shortens the carbon diffusion distance, consumes carbon more uniformly, and reduces the chance for a few graphite particles to grow into chunky colonies. This supports the trial 2 result because the antimony addition and rare earth control produced a higher nodule count in the thick section.
The matrix structure also changed slightly. The optimized process maintained the QT450 requirement. I did not observe an unacceptable increase in pearlite or carbide formation at 0.015% Sb. However, I kept the Sb addition under strict control because the window is narrow. The final acceptance criteria are listed in Table 12.
| Quality item | Acceptance criterion | Sampling location | Method |
|---|---|---|---|
| Chunky graphite area | Below minimum detectable level | Thick hot spot | Metallographic image analysis |
| Nodularity | Meets QT450 design requirement | Thick and thin sections | Optical microscopy |
| Nodule count | Sufficient and uniform | Thick hot spot | Image analysis |
| Graphite shape | No fragmented or branched colonies | Thick hot spot | Metallographic inspection |
| Matrix | QT450 specified ferrite-pearlite balance | Representative section | Microscopy and hardness |
| Sb content | Controlled near target | Pouring ladle | Optical emission spectroscopy |
| RE content | Low and controlled | Pouring ladle | Optical emission spectroscopy |
| Residual Mg | Within spheroidization window | Pouring ladle | Optical emission spectroscopy |
The final mechanism can be summarized as follows. In a thick-section ductile iron casting, the cooling rate is low and the solidification time is long. The long solidification time allows Ce and La to segregate to austenite grain boundaries. The rare earth-rich boundaries delay the closure of the austenite shell around the graphite. Carbon diffuses along the remaining liquid channels, and graphite grows as chunky or fragmented colonies. Removing rare earth from the cored wire alone is not enough because the thick-section thermal condition still favors degeneration. Adding a small amount of Sb changes the grain-boundary chemistry and interfacial conditions. Sb competes with rare earth elements, reduces their effective segregation, and helps maintain a higher nodule count. The result is nodular graphite instead of chunky graphite. The process window is narrow, so both rare earth and antimony must be controlled together with residual magnesium, inoculation, and local cooling.
I also prepared a summary of the key process changes and their effects. This summary is given in Table 13. It is useful for training and for future thick-section ductile iron casting projects.
| Change | Original condition | Optimized condition | Metallurgical effect |
|---|---|---|---|
| Rare earth in cored wire | Present | Reduced or eliminated | Less Ce and La grain-boundary segregation |
| Antimony addition | None | About 0.015% | Balances rare earth and refines graphite |
| Residual Mg | Sometimes high | Controlled window | Reduces excess freezing range |
| Inoculation | Standard | Strong late inoculation | Increases nodule count |
| Thermal control | Hot spot uncontrolled | Riser and cooling optimized | Reduces solidification time |
| Quality sampling | General section | Thick hot spot separately | Detects local chunky graphite |
In my final assessment, the chunky graphite defect in the thick-section ductile iron casting was solved by a combined chemical and thermal strategy. The most important chemical change was the use of a rare-earth-free or low-rare-earth magnesium-silicon-iron cored wire. The most important balancing addition was antimony at approximately 0.015%. The most important thermal understanding was that the thick center solidifies slowly and therefore has a much higher risk than the thin wall. The most important quality lesson was that local sampling is necessary because a ductile iron casting can have good graphite in one region and severe chunky graphite in another. With these measures, the black patches disappeared, the nodularity improved, and the thick-section ductile iron casting met the QT450 metallographic requirement.
The optimized process has been applied to subsequent production. I continue to monitor the residual magnesium, rare earth, and antimony contents, and I verify the thick-section microstructure by periodic dissection. The process is stable when the balance parameter is kept within the validated window. If the rare earth content increases unexpectedly, the risk of chunky graphite rises. If the antimony content becomes too high, the matrix may become too hard or carbides may appear. Therefore, the control plan treats the ductile iron casting as a coupled system of melting, spheroidization, inoculation, pouring, solidification, and local cooling. This is the approach I now use for all heavy-section ductile iron casting developments.
For future work, I recommend expanding the database of thick-section trials, measuring the local cooling rate more precisely, and coupling the chemical balance model with thermal simulation. A more general model can be written as
$$A_{CG} = f\left(w_{RE}, w_{Sb}, w_{Mg}, t_s, N_n, \dot{T}\right)$$
and the optimized condition can be expressed as
$$\min A_{CG} \quad \text{subject to} \quad \text{QT450 matrix and nodularity constraints}.$$
This formulation keeps the focus on the practical requirement: a sound ductile iron casting with nodular graphite, acceptable matrix, and no chunky graphite in the thick section. The work has shown that rare earth control alone is insufficient, and that a small, carefully controlled antimony addition can balance the harmful segregation of Ce and La. The result is a robust process for heavy-section ductile iron castings such as the hydraulic rear cover.