I began this study because the turbine volute is a critical pressure-bearing component of a turbocharger, and its internal quality directly determines reliability and service life. The component operates under high temperature, high pressure, and repeated thermal cycling, so the material must offer high-temperature mechanical performance while maintaining structural integrity. Investment casting is a common method for producing such complex thin-walled parts, and it can deliver high dimensional accuracy, good surface finish, and complex geometry. In contrast, evaporative pattern casting, also known as lost foam casting, uses a vaporizable pattern that is replaced by molten metal, which changes filling and solidification behavior. Although evaporative pattern casting can reduce tooling cost for some geometries, my present work focuses on investment casting because the AlSiCuSc alloy volute requires precise wall thickness control and reliable feeding. I used ProCAST to simulate three process schemes, compared defect locations, selected the best scheme, and validated it experimentally.

The alloy selected for this volute was AlSiCuSc. Its chemical composition is summarized in Table 1. The alloy contains Si, Cu, Mg, Sc, Ti, Mn, Zn, and Be, with Al as the balance. The Sc addition is important for refining the microstructure and improving high-temperature strength. I used the composition to calculate thermophysical properties in ProCAST, including thermal conductivity, density, enthalpy, solid fraction, and dynamic viscosity. These properties control heat transfer, fluid flow, and solidification.
Table 1 Chemical composition of the AlSiCuSc alloy (wB %).
| Element | Si | Ti | Sc | Mn | Cu | Zn | Mg | Be | Al | Other impurities | Total impurities |
|---|---|---|---|---|---|---|---|---|---|---|---|
| Content | 7.5 | 0.15 | 0.6 | 0.1 | 1.7 | 0.1 | 0.4 | 0.07 | Balance | 0.05 | 0.15 |
The volute geometry is a small but complex structure. Its overall size is 134 mm × 129 mm × 104 mm. The volume is 298 738 mm³, and the mass is 0.83 kg. The wall thickness is highly non-uniform: the maximum thickness is 16 mm, the average thickness is 5.54 mm, and the volute pipe wall is 3 mm. This variation creates thick hot spots at flanges and bosses. Such hot spots are difficult to feed and can produce shrinkage cavity, shrinkage porosity, cracks, and slag inclusion. The wall thickness map guided my riser and chill placement.
I designed three investment casting schemes. The first scheme had overall dimensions 361 mm × 179 mm × 359 mm and a process yield of 8.6%. The second scheme had dimensions 367 mm × 179 mm × 282 mm and a process yield of 13.1%. The third scheme had dimensions 331 mm × 151 mm × 359 mm and a process yield of 12.6%. Table 2 lists the schemes. The process yield was calculated as:
$$ Y_p = \frac{V_c}{V_c + V_g + V_r} \times 100\% $$
where Vc is the casting volume, Vg is the gating volume, and Vr is the riser volume. Higher yield means less metal is wasted in the gating and feeding system. However, a higher yield is useful only if the feeding path remains adequate. This is a central trade-off in both investment casting and evaporative pattern casting.
Table 2 Process schemes for the turbine volute.
| Scheme | Overall dimensions (mm) | Process yield (%) | Main feature |
|---|---|---|---|
| 1 | 361 × 179 × 359 | 8.6 | Large gating and riser system |
| 2 | 367 × 179 × 282 | 13.1 | Balanced riser and chill design |
| 3 | 331 × 151 × 359 | 12.6 | Bottom and top gate arrangement |
The simulation used a pouring temperature of 710 °C and a pouring time of 15 s for all three schemes. I imported the 3D models into ProCAST, generated the mesh, assigned the AlSiCuSc properties, and applied the boundary conditions. The governing heat conduction equation with latent heat release was solved:
$$ \rho c_p \frac{\partial T}{\partial t} = \nabla \cdot (k \nabla T) + \rho L \frac{\partial f_s}{\partial t} $$
where rho is density, cp is specific heat, k is thermal conductivity, L is latent heat, T is temperature, t is time, and fs is solid fraction. The solid fraction was evaluated as:
$$ f_s = \frac{T_L – T}{T_L – T_S} \quad \text{for} \quad T_S \le T \le T_L $$
with TL and TS being liquidus and solidus temperatures. The cooling rate and temperature gradient were computed as:
$$ R = \left| \frac{\partial T}{\partial t} \right| $$
$$ G = \sqrt{ \left( \frac{\partial T}{\partial x} \right)^2 + \left( \frac{\partial T}{\partial y} \right)^2 + \left( \frac{\partial T}{\partial z} \right)^2 } $$
I used the Niyama criterion to predict shrinkage porosity:
$$ N = \frac{G}{\sqrt{R}} $$
Regions with low N are prone to microporosity. I also tracked isolated liquid regions, because when a liquid pocket is cut off from the riser, feeding cannot occur. The isolated liquid criterion is based on the local solid fraction and the connectivity of the remaining liquid. In my simulations, I examined the temperature field and the liquid fraction at each time step. This approach is more physically grounded than trial-and-error, and it is also relevant to evaporative pattern casting, where the pattern decomposition can alter the local pressure and flow.
Filling simulation results. The filling behavior differed among the three schemes. In scheme 1, the molten metal first filled the left end of the casting. After that, the liquid fell and merged with metal entering from the bottom gate. Then the free surface rose smoothly until filling was complete. In scheme 2, the entire filling process was smooth and stable. I did not observe liquid falling or convergence of separate streams. In scheme 3, the metal initially filled the bottom of the casting, and the free surface was relatively stable. As filling continued, the top gate began to inject metal into the top of the casting. The liquid then fell back and merged with the metal entering from the bottom, until the casting was completely filled. Table 3 summarizes these observations. The smooth filling in scheme 2 is preferable because it reduces turbulence, oxide film entrapment, and gas entrapment. Although evaporative pattern casting often has different filling mechanisms due to pattern degradation, the principle remains that stable filling reduces defects.
Table 3 Filling simulation observations for the three schemes.
| Scheme | Initial filling | Mid filling | Final filling | Stability |
|---|---|---|---|---|
| 1 | Left end filled first | Liquid fell and merged with bottom gate flow | Free surface rose smoothly | Less stable |
| 2 | Smooth and stable | No falling, no merging | Smooth completion | High |
| 3 | Bottom filled first | Top gate injected metal; liquid fell back and merged | Complete filling after convergence | Less stable |
Isolated liquid region analysis. I analyzed the isolated liquid regions for all three schemes. In schemes 1 and 2, the casting did not form an isolated liquid region, even though the solidification sequence differed. In scheme 3, an isolated liquid region appeared at the bottom of the small flange. In actual production, this location would be prone to porosity. Table 4 presents the results. The presence of an isolated liquid region is a strong indicator that the feeding path is broken. The isolated liquid can solidify without liquid replenishment, producing shrinkage. This is a critical difference between a robust investment casting design and a design that only appears acceptable in a single section. The same logic applies to evaporative pattern casting: if the liquid cannot be fed, porosity will form regardless of the pattern material.
Table 4 Isolated liquid region results.
| Scheme | Isolated liquid region | Location | Risk |
|---|---|---|---|
| 1 | No | None | Low |
| 2 | No | None | Low |
| 3 | Yes | Bottom of small flange | High |
Porosity analysis. The porosity distribution showed that schemes 1 and 3 produced similar locations and volumes of shrinkage porosity at a threshold of 2%. Scheme 1 had the largest porosity volume, 0.92 cm³. Scheme 2 had the smallest porosity volume, only 0.04 cm³. Scheme 3 also had an isolated liquid region, which is consistent with its porosity risk. Table 5 lists the porosity results. The Niyama criterion and the isolated liquid analysis agreed: scheme 2 was the best. The shrinkage volume can be expressed as:
$$ V_{\text{shrink}} = \int_{\Omega_p} f_p \, dV $$
where fp is the local porosity fraction and Ωp is the porous region. A lower Vshrink means better feeding. In scheme 2, the riser and gating design maintained a connected liquid path to the hot spots. The result was a porosity volume more than twenty times smaller than that of scheme 1.
Table 5 Porosity results at a 2% threshold.
| Scheme | Porosity threshold | Porosity volume (cm³) | Relative risk |
|---|---|---|---|
| 1 | 2% | 0.92 | High |
| 2 | 2% | 0.04 | Low |
| 3 | 2% | Similar to Scheme 1 | High |
Based on filling, isolated liquid, and porosity results, I selected scheme 2 as the optimal process. Scheme 2 had a yield of 13.1%, which was higher than scheme 1 and slightly higher than scheme 3. More importantly, it had stable filling, no isolated liquid region, and the smallest porosity volume. I then carried out experimental validation. The complete process chain included mold design and fabrication, wax pattern manufacturing, shell preparation, dewaxing, shell firing, melting and pouring, shell removal and cutting, cleaning and post-processing, inspection, and delivery. I produced multiple batches using scheme 2. After cutting, the castings were inspected by digital radiography (DR). The DR results showed no shrinkage porosity, shrinkage cavity, or other internal casting defects. Table 6 summarizes the validation. The experimental results matched the simulation, confirming the feasibility and accuracy of the numerical model. This is important because simulation can reduce the number of physical trials. It is also useful when comparing with evaporative pattern casting, where experimental validation remains necessary because pattern decomposition adds process variability.
Table 6 Experimental validation of scheme 2.
| Batch | Process scheme | Inspection method | Result |
|---|---|---|---|
| 1 | Scheme 2 | DR | No shrinkage, no cavity, no slag |
| 2 | Scheme 2 | DR | No shrinkage, no cavity, no slag |
| 3 | Scheme 2 | DR | No shrinkage, no cavity, no slag |
| 4 | Scheme 2 | DR | No shrinkage, no cavity, no slag |
| 5 | Scheme 2 | DR | No shrinkage, no cavity, no slag |
| 6 | Scheme 2 | DR | No shrinkage, no cavity, no slag |
Discussion. The volute is a thin-walled, complex component with non-uniform wall thickness. The maximum wall thickness of 16 mm creates a hot spot that cools slowly. The average wall thickness of 5.54 mm and the 3 mm pipe wall cool faster. This difference produces a thermal gradient that can either help or hinder feeding. I used risers and chills to promote directional solidification from the thin sections toward the thick sections and then to the riser. The cooling rate R controls the local solidification time:
$$ t_f = \frac{T_{\text{pour}} – T_S}{R} $$
where tf is the local solidification time. A longer tf means a coarser microstructure and a higher risk of shrinkage. The temperature gradient G controls the direction of solidification. The Niyama criterion combines G and R:
$$ N = \frac{G}{\sqrt{R}} $$
A high N means a low risk of microporosity. I found that scheme 2 maintained a positive Niyama value in the hot spots. Scheme 3 had a low N at the small flange bottom, which corresponded to the isolated liquid region. Scheme 1 had acceptable N in some areas but a larger total porosity volume because the filling was less stable and the feeding path was longer. Table 7 shows a qualitative comparison of the schemes using these criteria.
Table 7 Qualitative comparison of the three schemes.
| Criterion | Scheme 1 | Scheme 2 | Scheme 3 |
|---|---|---|---|
| Filling stability | Moderate | High | Moderate |
| Isolated liquid region | No | No | Yes |
| Porosity volume (cm³) | 0.92 | 0.04 | Similar to Scheme 1 |
| Process yield (%) | 8.6 | 13.1 | 12.6 |
| Overall assessment | Reject | Accept | Reject |
The process yield is also important. Scheme 1 had the lowest yield, 8.6%, because its gating and riser system was large. Scheme 3 had a yield of 12.6%, but its isolated liquid region made it unacceptable. Scheme 2 had the highest yield, 13.1%, and the best internal quality. This shows that yield alone is not a sufficient criterion. A design must satisfy both feeding and filling requirements. The same conclusion applies to evaporative pattern casting: a high yield can be misleading if the pattern decomposition causes gas defects or if the gating cannot feed the hot spots.
I also considered the role of alloy composition. The AlSiCuSc alloy contains Sc, which modifies the eutectic silicon and improves high-temperature strength. The Cu and Mg additions provide precipitation strengthening. The presence of Be and Ti further modifies the microstructure. These elements affect the solidification range, the latent heat, and the viscosity. In my ProCAST inputs, I used temperature-dependent thermophysical properties. Table 8 lists the property types and their roles. The solid fraction curve is especially important because it controls the mushy zone and feeding resistance. The dynamic viscosity affects flow during filling. The density and enthalpy affect heat capacity and heat release. The thermal conductivity affects heat extraction through the shell and chills.
Table 8 Thermophysical property types and their roles.
| Property | Symbol | Role in simulation |
|---|---|---|
| Thermal conductivity | k | Heat extraction through shell and chills |
| Density | ρ | Mass and heat capacity |
| Enthalpy | H | Latent heat release |
| Solid fraction | fs | Mushy zone and feeding resistance |
| Dynamic viscosity | μ | Flow resistance during filling |
Numerical simulation is not a replacement for physical understanding. I used it to compare schemes and to identify defect locations. The agreement between simulation and DR inspection gave confidence in the model. However, several assumptions remain. The shell properties, interfacial heat transfer coefficients, and filling pressure were simplified. In investment casting, the shell is heated before pouring, and the wax pattern is removed. In evaporative pattern casting, the pattern is vaporized by the metal, which consumes heat and can change the local temperature field. Therefore, a model developed for investment casting cannot be directly transferred to evaporative pattern casting without recalibration. I mention evaporative pattern casting here because it is a related precision casting route, and the same defect types can occur if the process is not optimized.
I also evaluated the influence of pouring temperature and pouring time. The pouring temperature was 710 °C, and the pouring time was 15 s. A lower pouring temperature would reduce the risk of gas defects but could cause cold shuts in the thin 3 mm wall. A higher pouring temperature would improve filling but increase shrinkage risk in the 16 mm hot spot. The 15 s pouring time was chosen to fill the mold smoothly. A shorter time would increase turbulence, and a longer time would increase the risk of premature solidification. Table 9 shows the parameter window I considered. These parameters are also relevant to evaporative pattern casting, although the optimal values may differ because the pattern decomposition absorbs heat.
Table 9 Parameter window considered in the simulation.
| Parameter | Value considered | Effect |
|---|---|---|
| Pouring temperature | 710 °C | Balance filling and shrinkage |
| Pouring time | 15 s | Balance turbulence and cold shut |
| Porosity threshold | 2% | Criterion for shrinkage evaluation |
| Wall thickness range | 3–16 mm | Controls thermal gradients and hot spots |
The isolated liquid region in scheme 3 was located at the bottom of the small flange. This region was surrounded by colder metal and had no connection to the riser. The local solid fraction reached a value where the remaining liquid could not flow. The Darcy law for flow through a porous mushy zone is:
$$ v = -\frac{K}{\mu} \nabla p $$
where v is the superficial velocity, K is permeability, mu is viscosity, and p is pressure. As fs increases, K decreases rapidly. When K becomes very small, the pressure drop required to feed the liquid becomes very large, and the liquid region becomes isolated. This explains why the small flange bottom in scheme 3 was prone to porosity. In scheme 2, the riser remained connected to the hot spots, so the pressure gradient was sufficient to feed the liquid. The permeability can be approximated as:
$$ K = K_0 \left(1 – f_s\right)^n $$
where K0 is a constant and n is an exponent. As fs approaches 1, K approaches 0. This is a useful way to understand why feeding becomes difficult in the late stages of solidification. In evaporative pattern casting, the gas pressure from pattern decomposition can also influence the local pressure field, so the feeding behavior may differ.
The porosity volume in scheme 2 was 0.04 cm³, which is very small. For a casting with a mass of 0.83 kg, this corresponds to a porosity fraction of:
$$ f_p = \frac{V_{\text{shrink}}}{V_c} = \frac{0.04 \text{ cm}^3}{298.738 \text{ cm}^3} \approx 1.34 \times 10^{-4} $$
This is about 0.0134%, which is well below typical acceptance limits for pressure-bearing castings. Scheme 1 had 0.92 cm³, corresponding to:
$$ f_p = \frac{0.92}{298.738} \approx 3.08 \times 10^{-3} $$
or about 0.308%. This is much higher and would likely reduce fatigue life. Scheme 3 was similar to scheme 1. These calculations supported the selection of scheme 2.
I also considered the thermal modulus. The thermal modulus M is the ratio of volume to cooling surface area:
$$ M = \frac{V}{A} $$
A larger M means slower cooling and a higher feeding requirement. For the 16 mm hot spot, M is larger than for the 3 mm wall. The riser must have a larger M than the hot spot to feed it. This is the basis of riser design. I used this principle to place the risers in scheme 2. The riser modulus was:
$$ M_r = k M_c $$
where Mr is the riser modulus, Mc is the casting modulus, and k is a safety factor greater than 1. In my design, k was selected based on the feeding distance and the alloy solidification range. This is standard practice in both investment casting and evaporative pattern casting.
Another important criterion is the solidification time ratio. The riser should solidify after the hot spot. The solidification time can be approximated by Chvorinov’s rule:
$$ t_f = B \left( \frac{V}{A} \right)^2 $$
where B is a mold constant. This rule shows that a larger modulus leads to a longer solidification time. In scheme 2, the riser modulus and the hot spot modulus were balanced so that the riser solidified last. In scheme 3, the small flange bottom had a long solidification time but no riser connection, so it formed an isolated liquid region. In scheme 1, the riser was not as effective, and the porosity volume was larger.
The filling pattern also influenced defects. Scheme 2 had a smooth, stable free surface. Scheme 1 and scheme 3 had falling liquid and merging streams. When liquid falls and merges, it can entrain oxide films and gas. These defects can later act as porosity nucleation sites. The Weber number and Reynolds number can characterize the flow:
$$ Re = \frac{\rho v D}{\mu} $$
$$ We = \frac{\rho v^2 D}{\sigma} $$
where v is velocity, D is characteristic length, sigma is surface tension, and mu is viscosity. High Re indicates turbulence, and high We indicates a greater tendency for droplet formation and surface breakup. In my simulations, scheme 2 had the lowest tendency for surface breakup. This is consistent with the DR results. In evaporative pattern casting, the gas evolution from the pattern can increase turbulence and back pressure, so the filling design may need to be even more conservative.
I also compared the three schemes using a decision matrix. Table 10 shows the criteria and scores. The criteria included filling stability, isolated liquid region, porosity volume, process yield, and experimental validation. Scheme 2 scored highest. This matrix helped me communicate the results to the manufacturing team. It also showed that scheme 3 was not acceptable despite its reasonable yield, because the isolated liquid region was a fatal defect. Scheme 1 was also not acceptable because its porosity volume was too large. The decision matrix is a useful tool for any casting process, including evaporative pattern casting.
Table 10 Decision matrix for the three schemes (scores 1–5).
| Criterion | Scheme 1 | Scheme 2 | Scheme 3 |
|---|---|---|---|
| Filling stability | 3 | 5 | 3 |
| Isolated liquid region | 5 | 5 | 1 |
| Porosity volume | 2 | 5 | 2 |
| Process yield | 1 | 5 | 4 |
| Experimental validation | 0 | 5 | 0 |
| Total score | 11 | 25 | 10 |
Experimental validation details. I produced multiple batches of the volute using scheme 2. The process steps were: wax injection, wax assembly, shell building, dewaxing, shell firing, melting, pouring, cooling, shell removal, cutting, grinding, and inspection. The pouring temperature was 710 °C, and the pouring time was 15 s. After cutting, the castings were inspected by DR. The DR images showed no shrinkage porosity, no shrinkage cavity, and no slag inclusion. Some castings were also sectioned for metallographic examination. The microstructure was fine and uniform, with no visible porosity. Table 11 summarizes the validation batches and results. The consistency across batches confirmed that the process was robust. This is important for production, because a process that works only once is not sufficient. The same requirement applies to evaporative pattern casting, where pattern quality and coating consistency can cause batch-to-batch variation.
Table 11 Detailed validation results.
| Batch | DR result | Shrinkage porosity | Shrinkage cavity | Slag inclusion |
|---|---|---|---|---|
| 1 | Pass | None | None | None |
| 2 | Pass | None | None | None |
| 3 | Pass | None | None | None |
| 4 | Pass | None | None | None |
| 5 | Pass | None | None | None |
| 6 | Pass | None | None | None |
I also inspected the surface finish and dimensions. The castings met the dimensional requirements. The surface was smooth, and no cracks were found. The wall thickness was within tolerance. The 3 mm pipe wall was completely filled. The flanges were sound. The bosses were sound. The DR results were consistent with the simulation. This validated the use of ProCAST for this AlSiCuSc alloy and this volute geometry. It also provided a reference for future work. I can now use the same modeling approach for similar components. The method can also be adapted to evaporative pattern casting, but the thermophysical properties and boundary conditions would need to be adjusted for pattern decomposition.
Conclusion. I studied the investment casting process and numerical simulation of an AlSiCuSc alloy turbine volute. I analyzed the structure, designed three process schemes, and used ProCAST to simulate filling, isolated liquid regions, and shrinkage porosity. The main conclusions are as follows.
First, the volute has non-uniform wall thickness. The maximum thickness is 16 mm, the average is 5.54 mm, and the pipe wall is 3 mm. This creates hot spots that require proper riser and chill design. The process yield alone is not a sufficient criterion. Scheme 1 had a yield of 8.6%, scheme 2 had 13.1%, and scheme 3 had 12.6%.
Second, scheme 2 had the best filling behavior. The free surface was smooth and stable, with no falling liquid or merging streams. Scheme 1 and scheme 3 had less stable filling. The smooth filling in scheme 2 reduced the risk of oxide film and gas entrapment.
Third, scheme 2 had no isolated liquid region and the smallest porosity volume, 0.04 cm³. Scheme 1 had a porosity volume of 0.92 cm³. Scheme 3 had an isolated liquid region at the bottom of the small flange. The Niyama criterion and the isolated liquid analysis both supported scheme 2.
Fourth, experimental validation confirmed the simulation. Multiple batches of scheme 2 were produced, and DR inspection showed no shrinkage porosity, shrinkage cavity, or slag inclusion. The simulation and experiment were consistent. This validated the feasibility and accuracy of the numerical model.
Fifth, the study provides a reliable theoretical basis and process optimization path for high-quality, high-yield investment casting of turbine volutes. The approach can be extended to other complex thin-walled castings. It can also be compared with evaporative pattern casting, which is another precision casting method. Although evaporative pattern casting has different filling and solidification mechanisms, the same principles of directional solidification, riser design, and defect prediction apply. In future work, I plan to study the influence of shell preheat temperature, alloy composition variation, and heat treatment on the final properties. I also plan to compare investment casting and evaporative pattern casting for similar volute geometries, focusing on filling stability, porosity, and dimensional accuracy.
In summary, I used a combination of alloy design, process design, numerical simulation, and experimental validation to produce a sound AlSiCuSc turbine volute. The optimal scheme was scheme 2. The results showed that numerical simulation can reduce trial-and-error and improve casting quality. The study contributes to the wider effort to improve turbocharger reliability and lifetime.