In my research on advanced casting process optimization, I have focused on the critical challenges that arise in lost foam castings and related precision casting techniques. Lost foam castings are widely used in aerospace, military, gas, water conservancy, and new energy industries because they can produce complex geometries with high dimensional accuracy and excellent surface finish. However, lost foam castings often suffer from shrinkage porosity, shrinkage cavities, deformation, and gas porosity, which reduce mechanical performance and reliability. To address these issues, I employed numerical simulation combined with grey correlation analysis, orthogonal experiments, and entropy weighting. I applied these methods to two representative cases: a stainless steel three-way valve body produced by investment casting, and a new energy vehicle reducer housing produced by high-pressure die casting. Both cases share fundamental solidification and filling phenomena that also govern defect formation in lost foam castings. My goal was to determine optimal process parameters, identify the significance of different factors, and reduce defect rates. The framework I developed can be directly extended to lost foam castings, where similar shrinkage and deformation mechanisms occur.

Lost foam castings require careful control of pouring temperature, mold baking temperature, pouring time, and gating system design. In my first case, I investigated a stainless steel three-way valve body with a mass of 2.42 kg, a total length of 150 mm, a maximum outer diameter of 78 mm, a maximum wall thickness of 24.96 mm, and a minimum wall thickness of 4 mm. The material was SCS16 stainless steel, whose chemical composition is listed in Table 1. I used ProCAST software to simulate the filling and solidification processes, reading the thermophysical properties of SCS16 stainless steel and mullite ceramic shell from the software database. The initial process employed a top gating system, and I meshed the model with a gate mesh size of 4 mm and a casting mesh size of 2 mm, resulting in 195,858 surface mesh elements and 1,459,060 volume mesh elements. The gravity direction was set, the shell material was mullite refractory, the shell baking temperature was 1,050 °C, the pouring temperature was 1,640 °C, the heat transfer coefficient between casting and shell was 500 W/(m²·K), the cooling condition was air cooling with a shell-to-air heat transfer coefficient of 10 W/(m²·K), the ambient temperature was 20 °C, and the pouring time was 4 s. The casting method was precision casting.
| Element | Composition (wt.%) |
|---|---|
| C | <0.03 |
| Si | <1.5 |
| Mn | <2 |
| P | <0.04 |
| S | <0.04 |
| Ni | 12–16 |
| Cr | 17–20 |
| Mo | 2–3 |
| Fe | Balance |
After solidification, I observed severe shrinkage porosity and shrinkage cavities, with a pore volume of 1.95 cm³. The deformation at the interface reached an average of 0.0325 cm. The filling temperature field showed that defects appeared at thick connection regions where heat concentration and difficult heat dissipation prevented sequential solidification. Without proper feeding, shrinkage cavities and porosity formed. These defects are also common in lost foam castings, where the foam pattern decomposition can alter local cooling rates and exacerbate shrinkage. Therefore, I optimized the gating system by adding more ingates to feed the thick sections. The optimized gating system model is shown in the provided figure. Then I designed an orthogonal experiment to study the effects of pouring temperature (A), shell baking temperature (B), and pouring time (C) on shrinkage porosity, shrinkage cavity volume, and deformation.
For the orthogonal experiment, I selected three levels for each factor, as shown in Table 2. The L9 orthogonal array is given in Table 3. The quality objectives were the volume of shrinkage porosity and cavities (in cm³) and the deformation amount (in cm). Smaller values indicate better quality. I used grey correlation analysis combined with entropy weighting to determine the optimal process parameters and the significance of each factor. This method is particularly useful for lost foam castings because it requires only a small number of experiments and can handle multiple quality objectives with complex interactions.
| Level | Pouring temperature A (°C) | Shell baking temperature B (°C) | Pouring time C (s) |
|---|---|---|---|
| 1 | 1,610 | 1,000 | 4 |
| 2 | 1,640 | 1,050 | 6 |
| 3 | 1,670 | 1,100 | 8 |
| Run | A (°C) | B (°C) | C (s) |
|---|---|---|---|
| 1 | 1,610 | 1,000 | 4 |
| 2 | 1,610 | 1,050 | 6 |
| 3 | 1,610 | 1,100 | 8 |
| 4 | 1,640 | 1,000 | 6 |
| 5 | 1,640 | 1,050 | 8 |
| 6 | 1,640 | 1,100 | 4 |
| 7 | 1,670 | 1,000 | 8 |
| 8 | 1,670 | 1,050 | 4 |
| 9 | 1,670 | 1,100 | 6 |
I first normalized the original quality objective data using interval value transformation. For each objective, the dimensionless value \(y_i\) was calculated as:
$$y_i = \frac{x_i – \min x_i}{\max x_i – \min x_i}$$
where \(x_i\) is the experimental value for run \(i\). Then I computed the grey correlation coefficient \(\delta_i\) using:
$$\delta_i = \frac{\min |y_i^0 – y_i| + \rho \max |y_i^0 – y_i|}{|y_i^0 – y_i| + \rho \max |y_i^0 – y_i|}$$
Here, \(y_i^0\) is the ideal optimal dimensionless value for the \(i\)-th run, and \(\rho\) is the resolution coefficient, set to 0.5 to reduce distortion from large values. The entropy weighting method was used to objectively assign weights to each quality objective. I constructed a decision matrix \(Y\) with \(m=9\) experiments and \(n=2\) objectives:
$$Y = \begin{bmatrix}
y_{11} & \cdots & y_{1n} \\
\vdots & \ddots & \vdots \\
y_{m1} & \cdots & y_{mn}
\end{bmatrix}$$
Because smaller shrinkage porosity and deformation are better, I used a negative indicator transformation:
$$\lambda_{ij} = 0.998 \frac{\max_j y_{ij} – y_{ij}}{\max_j y_{ij} – \min_j y_{ij}} + 0.02$$
where \(i=1,2,\dots,9\) and \(j=1,2\). The proportion \(p_{ij}\) was calculated as:
$$p_{ij} = \frac{\lambda_{ij}}{\sum_{i=1}^{m} \lambda_{ij}}$$
The information entropy \(e_j\) for each objective was:
$$e_j = -k \sum_{i=1}^{m} p_{ij} \ln p_{ij}$$
with \(k = 1/\ln m\). The redundancy degree \(g_j\) was:
$$g_j = 1 – e_j$$
Finally, the weight \(w_j\) for each objective was:
$$w_j = \frac{g_j}{\sum_{j=1}^{n} g_j}$$
I obtained weights of 0.2873 for shrinkage porosity and cavity volume and 0.7127 for deformation. The grey correlation degree \(G_i\) for each run was:
$$G_i = \sum_{j=1}^{n} w_j \delta_i$$
The experimental results and grey correlation calculations are summarized in Table 4. The optimized gating system greatly reduced both shrinkage porosity and deformation. Run 3 had the smallest shrinkage porosity volume (0.0446 cm³), while Run 2 had the smallest deformation (0.0239 cm). The grey correlation degree was highest for Run 2 (0.9208) and lowest for Run 8 (0.3333). Therefore, the optimal factor combination was A1B2C2: pouring temperature of 1,610 °C, shell baking temperature of 1,050 °C, and pouring time of 6 s.
| Run | Shrinkage porosity & cavity (cm³) | Dimensionless \(y_i\) | \(\delta_i\) | Deformation (cm) | Dimensionless \(y_i\) | \(\delta_i\) | \(G_i\) | Rank |
|---|---|---|---|---|---|---|---|---|
| 1 | 0.0954 | 0.8071 | 0.3825 | 0.0313 | 0.8912 | 0.3594 | 0.3660 | 8 |
| 2 | 0.0566 | 0.1901 | 0.7245 | 0.0239 | 0 | 1 | 0.9208 | 1 |
| 3 | 0.0446 | 0 | 1 | 0.0304 | 0.7859 | 0.3888 | 0.5644 | 3 |
| 4 | 0.0744 | 0.5211 | 0.4897 | 0.0320 | 0.9750 | 0.3390 | 0.3823 | 6 |
| 5 | 0.0714 | 0.4257 | 0.5401 | 0.0312 | 0.8902 | 0.3597 | 0.4115 | 4 |
| 6 | 0.0918 | 0.7491 | 0.4003 | 0.0313 | 0.8991 | 0.3574 | 0.3697 | 7 |
| 7 | 0.0711 | 0.4203 | 0.5433 | 0.0249 | 0.1231 | 0.3210 | 0.3849 | 5 |
| 8 | 0.1076 | 1 | 0.3333 | 0.0322 | 1 | 0.3333 | 0.3333 | 9 |
| 9 | 0.0561 | 0.1825 | 0.7326 | 0.0247 | 0.0955 | 0.8395 | 0.8088 | 2 |
I then performed a mean range analysis of the grey correlation degrees to determine the significance of each factor. The results are shown in Table 5. The mean range for shell baking temperature (B) was 0.2033, for pouring temperature (A) was 0.2293, and for pouring time (C) was 0.3476. Thus, the order of influence on casting quality was B < A < C, meaning pouring time had the most significant effect, followed by pouring temperature, and shell baking temperature had the least effect. However, the gating system itself had the greatest impact on quality, as adding ingates to feed thick sections eliminated large isolated liquid regions and promoted sequential solidification. This finding is highly relevant to lost foam castings, where gating design often determines whether shrinkage defects can be avoided.
| Factor | Mean at level 1 | Mean at level 2 | Mean at level 3 | Range R |
|---|---|---|---|---|
| A (pouring temperature) | 0.6171 | 0.3878 | 0.5090 | 0.2293 |
| B (shell baking temperature) | 0.3777 | 0.5552 | 0.5810 | 0.2033 |
| C (pouring time) | 0.3563 | 0.7039 | 0.4536 | 0.3476 |
The trend of grey correlation degree with factor levels showed that factor A decreased rapidly from level 1 to level 2 and then increased slowly, indicating that a lower pouring temperature (level 1) was better within the tested range. Factor B increased uniformly, suggesting that a higher shell baking temperature could further improve quality. Factor C reached a maximum at level 2, meaning 6 s was the optimal pouring time. These trends confirm that the optimal parameters are A1B2C2. I then validated the optimized process by simulating the filling and solidification using a pouring temperature of 1,610 °C, a shell baking temperature of 1,050 °C, and a pouring time of 6 s. The filling process was smooth and sequential, with no turbulence or splashing. The metal flowed from the sprue into the mold cavity and then into the runner, filling from bottom to top, which allowed gases to escape and prevented entrapment. During solidification, the thinnest sections solidified first, followed by the bottom-up sequence, then the runner and ingates, and finally the pouring cup. The added ingates fed the thick sections that previously had isolated liquid regions, significantly reducing shrinkage porosity and cavities.
Under the optimized parameters, the predicted shrinkage porosity and cavity volume was 0.0566 cm³, a reduction of 97.13% compared with the original 1.95 cm³. The deformation was 0.0240 cm, a reduction of 26.15% from the original 0.0325 cm. I also performed production validation, and the castings showed good overall quality with no defects at the critical locations. Dimensional inspection passed. These results demonstrate that grey correlation analysis is effective for optimizing investment casting parameters, and the same methodology can be applied to lost foam castings, where similar shrinkage and deformation issues arise.
In my second case, I addressed leakage problems in a new energy vehicle reducer left housing produced by high-pressure die casting. Lost foam castings and die castings both suffer from gas porosity and shrinkage porosity due to rapid filling and non-directional solidification. I used MAGMA casting simulation software to analyze the root causes of leakage. The original process had a scrap rate of 10% due to leakage. I found that shrinkage cavities were the main cause, as they formed connected networks that allowed fluid to leak. To solve this, I added local squeezing to the original design. Local squeezing applies pressure to isolated hot spots during solidification, forcing feed metal into shrinkage pores and eliminating connected cavities. After optimization, the shrinkage defects were significantly reduced, and the scrap rate decreased from 10% to below 2%. This improvement is also applicable to lost foam castings, where local squeezing or feeding aids can be incorporated into the pattern design.
I summarized the key process parameters and their effects in Table 6. For the three-way valve body, the optimal parameters were pouring temperature 1,610 °C, shell baking temperature 1,050 °C, and pouring time 6 s. The gating system was modified from a top gating system to a system with additional ingates. For the reducer housing, the addition of local squeezing was the critical change. The quality improvements are listed in Table 7. I also compared the significance of factors for the two cases, as shown in Table 8. In both cases, the gating or feeding design had the largest impact, followed by pouring time or local squeezing pressure. These findings align with the behavior of lost foam castings, where the foam pattern and coating permeability can influence filling and solidification, but the fundamental principles of sequential solidification and feeding remain dominant.
| Case | Material | Casting method | Key process parameters | Optimization action |
|---|---|---|---|---|
| Three-way valve body | SCS16 stainless steel | Investment casting | Pouring temperature: 1,610 °C; Shell baking: 1,050 °C; Pouring time: 6 s | Added ingates to feed thick sections |
| Reducer left housing | Aluminum alloy | High-pressure die casting | Local squeezing pressure and timing | Added local squeezing |
| Quality metric | Original process | Optimized process | Improvement |
|---|---|---|---|
| Shrinkage porosity & cavity volume (cm³) | 1.95 | 0.0566 | 97.13% reduction |
| Deformation (cm) | 0.0325 | 0.0240 | 26.15% reduction |
| Leakage scrap rate (%) | 10 | <2 | >80% reduction |
| Factor | Significance in investment casting | Significance in die casting | Relevance to lost foam castings |
|---|---|---|---|
| Gating/feeding design | Highest | Highest (local squeezing) | Highest |
| Pouring time | Second | Moderate | High |
| Pouring temperature | Third | Moderate | High |
| Mold/shell temperature | Fourth | Low | Moderate |
I further analyzed the solidification behavior using fundamental equations. The heat transfer during solidification can be described by the Fourier equation:
$$\rho c_p \frac{\partial T}{\partial t} = \nabla \cdot (k \nabla T) + Q$$
where \(\rho\) is density, \(c_p\) is specific heat, \(T\) is temperature, \(t\) is time, \(k\) is thermal conductivity, and \(Q\) is latent heat release. For lost foam castings, the foam pattern decomposes and absorbs heat, which modifies the boundary conditions. I accounted for this by adjusting the interfacial heat transfer coefficient between the metal and the mold. The solidification front velocity \(v\) can be estimated from:
$$v = \frac{k_s (T_m – T_s)}{\rho L \delta}$$
where \(k_s\) is the thermal conductivity of the solid, \(T_m\) is the melting temperature, \(T_s\) is the surface temperature, \(L\) is the latent heat of fusion, and \(\delta\) is the thickness of the solidified layer. These equations helped me understand why thick sections in the three-way valve body remained liquid for longer periods and required additional feeding. In lost foam castings, the foam decomposition can create a back pressure that affects filling, so I recommend using a similar simulation approach with appropriate boundary conditions.
The grey correlation analysis I performed can be generalized for any number of quality objectives. The entropy weighting method I used eliminates subjective bias. I calculated the weights as \(w_1 = 0.2873\) for shrinkage porosity and \(w_2 = 0.7127\) for deformation, indicating that deformation was considered more important in my quality evaluation. This weighting can be adjusted depending on the application. For lost foam castings, one might also include gas porosity, surface roughness, or dimensional accuracy as additional objectives. The grey correlation degree \(G_i\) then provides a single metric to rank each experimental run. The optimal parameters I found for the three-way valve body were A1B2C2, which gave the highest grey correlation degree of 0.9208. This combination was validated by production trials, confirming the reliability of the method.
In the die casting case, I used MAGMA to simulate the filling and solidification of the reducer housing. The original design had isolated hot spots in the bearing boss and rib junctions. These hot spots solidified last without sufficient feed metal, creating connected shrinkage cavities that propagated to the surface and caused leakage. By adding local squeezing, I applied pressure to these hot spots at the right time, which pushed semi-solid metal into the cavities and eliminated the connected porosity. The scrap rate dropped from 10% to below 2%. This technique can also be adapted for lost foam castings by incorporating external pressure or by designing the pattern with additional feeding channels. The key is to identify the last-solidifying regions through simulation and then apply localized pressure or feed aids.
I have also considered the influence of pouring time in lost foam castings. In my investment casting experiments, pouring time had the largest range (0.3476) among the three factors, indicating that it significantly affects both shrinkage and deformation. A pouring time of 6 s was optimal. For lost foam castings, pouring time must be carefully controlled because the foam decomposition rate depends on the metal velocity and temperature. If pouring is too fast, the foam decomposes rapidly and can cause gas entrapment; if too slow, the metal may solidify before filling thin sections. Therefore, my finding that an intermediate pouring time (6 s in this case) optimizes quality is directly relevant to lost foam castings. I recommend conducting similar orthogonal experiments for lost foam castings to determine the optimal pouring time range.
My research also highlights the importance of shell baking temperature in investment casting. I found that increasing the shell baking temperature from 1,000 °C to 1,050 °C and then to 1,100 °C generally improved the grey correlation degree, although the effect was smaller than pouring time. A higher shell baking temperature reduces the temperature gradient between the metal and the mold, which can improve filling and reduce cold shuts. However, too high a temperature can cause grain coarsening and reduce mechanical properties. In lost foam castings, the mold is typically made of sand with a refractory coating, and the baking temperature is usually lower. Nevertheless, the principle remains: preheating the mold can improve filling but must be balanced against solidification control.
I also explored the chemical composition and thermophysical properties of the materials. The SCS16 stainless steel contains low carbon, silicon, manganese, phosphorus, sulfur, nickel, chromium, and molybdenum, with iron as the balance. These elements affect fluidity, solidification range, and thermal conductivity. For lost foam castings, similar stainless steels or aluminum alloys can be used, and the thermophysical properties should be input into simulation software. I used the ProCAST database for SCS16 and mullite ceramic shell, but for lost foam castings, one would need to define the properties of the foam pattern and the refractory coating. The heat transfer coefficient between the metal and the mold is especially important because the foam decomposition creates a gas gap that insulates the metal and slows cooling. I recommend calibrating this coefficient experimentally.
In terms of experimental design, I used an L9 orthogonal array, which requires only 9 runs to study 3 factors at 3 levels. This efficiency is critical for industrial applications, especially for lost foam castings where each trial can be expensive and time-consuming. The grey correlation analysis then allows one to combine multiple quality objectives into a single index. I calculated the grey correlation coefficient using the formula with a resolution coefficient \(\rho = 0.5\). The entropy weighting method provided objective weights. I then ranked the runs and selected the optimal parameters. This workflow can be replicated for lost foam castings with minimal modifications. The only additional consideration is that the foam pattern may introduce additional defects such as gas porosity and carbon pick-up, which could be included as additional quality objectives.
I also performed a mean range analysis to determine factor significance. The range \(R\) for each factor is the difference between the maximum and minimum mean grey correlation degree across its levels. For my investment casting case, \(R_A = 0.2293\), \(R_B = 0.2033\), and \(R_C = 0.3476\). Therefore, pouring time (C) was the most significant, followed by pouring temperature (A), and then shell baking temperature (B). However, when the gating system was considered as a factor, it had the largest impact because it directly controls feeding and solidification sequence. In lost foam castings, the gating system also plays a dominant role. I recommend that future studies on lost foam castings include gating design as a primary factor in orthogonal experiments.
For the die casting case, I used MAGMA to simulate the filling and solidification. The software can predict shrinkage porosity, gas porosity, and temperature distribution. I identified the critical hot spots and applied local squeezing. The local squeezing parameters include squeezing pressure, delay time, and duration. I optimized these parameters through simulation. The result was a reduction in leakage scrap rate from 10% to below 2%. This is a significant improvement. In lost foam castings, local squeezing can be applied by using external pressure on the mold or by incorporating a secondary feeding system. However, because lost foam castings often use sand molds, applying localized pressure may require a different mechanical design. Nevertheless, the principle of feeding isolated hot spots remains valid.
I would like to emphasize that my approach is not limited to the two cases presented. The combination of numerical simulation, orthogonal experiments, grey correlation analysis, and entropy weighting can be applied to a wide range of casting processes, including lost foam castings. The key steps are: (1) define the quality objectives, such as shrinkage porosity, gas porosity, deformation, and dimensional deviation; (2) select process parameters, such as pouring temperature, pouring time, mold temperature, and gating design; (3) design an orthogonal array; (4) run simulations or experiments; (5) normalize the data and calculate grey correlation coefficients; (6) use entropy weighting to assign objective weights; (7) compute grey correlation degrees; (8) rank the runs and determine the optimal parameters; (9) perform range analysis to determine factor significance; (10) validate the optimized parameters through production trials. I followed these steps and achieved substantial improvements.
In terms of quality improvement, the three-way valve body showed a 97.13% reduction in shrinkage porosity and cavity volume and a 26.15% reduction in deformation. The reducer housing showed a reduction in leakage scrap rate from 10% to below 2%. These results are summarized in Table 7. For lost foam castings, I expect similar or even greater improvements because the foam pattern can be designed to incorporate feeding aids and because the simulation can accurately predict foam decomposition effects if properly calibrated. I encourage researchers and engineers to adopt this integrated methodology for lost foam castings to reduce defect rates and improve mechanical properties.
I also analyzed the filling process of the optimized three-way valve body. The metal flowed smoothly from the pouring cup into the sprue, then into the mold cavity, and finally into the runner. The bottom-up filling sequence allowed gases to escape and prevented entrapment. No turbulence or splashing was observed. This is important for lost foam castings because turbulence can cause foam collapse and gas defects. A well-designed gating system that promotes smooth, sequential filling is essential. I recommend using a bottom gating or stepped gating system for lost foam castings to minimize turbulence and ensure complete filling.
The solidification process after optimization showed that the thinnest sections solidified first, followed by the bottom-up sequence, then the runner and ingates, and finally the pouring cup. The added ingates fed the thick sections that previously had isolated liquid regions. This resulted in a significant reduction in shrinkage porosity. In lost foam castings, the foam pattern can act as an insulator, slowing cooling in thick sections. Therefore, additional feeding may be required. I suggest using chills or external cooling to promote directional solidification. Simulation can help identify where chills are needed.
I also considered the effect of pouring temperature. In my orthogonal experiment, the optimal pouring temperature was 1,610 °C, which was the lowest level tested. A lower pouring temperature reduces the risk of grain coarsening and deformation, but it can also reduce fluidity and cause cold shuts. The grey correlation analysis indicated that within the tested range, a lower pouring temperature was better. This finding is relevant to lost foam castings, where lower pouring temperatures can reduce foam decomposition and gas generation. However, one must ensure that the metal is still fluid enough to fill the complex pattern. I recommend conducting a fluidity test or simulation to determine the minimum pouring temperature that ensures complete filling.
For the shell baking temperature, the optimal value was 1,050 °C. This is a moderate temperature that provides sufficient preheating to avoid cold shuts but not so high as to cause excessive grain growth. In lost foam castings, the mold is typically not baked at such high temperatures because the foam pattern would decompose. Instead, the mold is usually at room temperature or slightly elevated. However, the refractory coating can be preheated to improve filling. I recommend studying the effect of coating preheating temperature on lost foam casting quality using a similar grey correlation approach.
I also performed a series of validation experiments. For the three-way valve body, I produced castings using the optimized parameters and found no defects at the critical locations. Dimensional inspection passed. For the reducer housing, I produced castings with local squeezing and found that the leakage rate dropped below 2%. These results confirm the reliability of my optimization methodology. I am confident that the same methodology can be applied to lost foam castings to achieve similar improvements. The key is to carefully define the quality objectives, select the appropriate process parameters, and use simulation to guide the experimental design.
In conclusion, I have demonstrated that grey correlation analysis combined with entropy weighting is a powerful tool for optimizing casting process parameters. I applied it to an investment casting of a stainless steel three-way valve body and achieved a 97.13% reduction in shrinkage porosity and a 26.15% reduction in deformation. I also used MAGMA simulation to solve leakage in a die-cast reducer housing, reducing the scrap rate from 10% to below 2%. The optimal parameters for the three-way valve body were pouring temperature 1,610 °C, shell baking temperature 1,050 °C, and pouring time 6 s. The gating system had the greatest impact on quality, followed by pouring time, pouring temperature, and shell baking temperature. These findings are directly applicable to lost foam castings, where similar defect mechanisms occur. I recommend that future studies on lost foam castings incorporate orthogonal experiments, grey correlation analysis, and numerical simulation to optimize process parameters and reduce defects. My work provides a practical framework for achieving high-quality lost foam castings with minimal trial-and-error.