Development of Large Thermal Power Low-Pressure Inner Cylinder Ductile Iron Castings

The development and application of ductile iron castings represent a significant advancement in the manufacturing of critical components for heavy industry. Ductile iron, as a key material within the family of high-strength cast irons, offers a superior combination of tensile strength, plasticity, toughness, damping capacity, and wear resistance compared to other cast irons. These properties have cemented its position as the material of choice for large, load-bearing structural components in sectors such as engineering machinery, energy equipment, and defense. This article details the comprehensive research and successful production process for a large-scale, low-pressure inner cylinder上半 for thermal power generation units, a prime example of applying ductile iron castings to replace traditional fabrication methods in core machinery parts.

This specific component operates under complex stress conditions within a high-temperature, pressurized environment, demanding exceptional material performance in terms of strength, toughness, and durability. Traditionally, such low-pressure inner cylinders were fabricated from welded carbon steel plates. However, advancements in ductile iron metallurgy and foundry technology have now enabled a successful material substitution. Utilizing monolithic ductile iron castings not only circumvents common issues associated with welded joints, such as quality inconsistencies and heat-treatment distortions, but also provides the final assembly with improved flow efficiency and reduced energy loss. Furthermore, the casting approach offers shorter manufacturing lead times and lower costs, presenting a compelling competitive advantage.

The successful production of such complex ductile iron castings requires meticulous planning and analysis. The upper half of the cylinder, the subject of this study, is a substantial component with an envelope dimension of 4,520 mm × 2,750 mm × 3,020 mm and a weight of 25 tonnes. Its structure is characterized by a nominal wall thickness of 40 mm and a massive flange at the horizontal joint (mid-plane) with a thickness of 210 mm. The internal geometry is exceptionally complex, featuring a volute-shaped steam passageway segmented by multiple internal diaphragms, creating numerous semi-enclosed, narrow cavities. This complexity presents significant challenges in core box design, core production, and mold assembly control. Furthermore, various heavy sections connect to the thinner main body, creating isolated hot spots that necessitate separate solidification analysis and targeted process measures to prevent internal shrinkage defects.

The material specification is QT400-18A, requiring thorough metallographic examination and mechanical property testing. The rough casting must adhere to dimensional tolerances per GB/T 6414-2017 CT12 grade. Non-destructive testing (NDT), including 100% magnetic particle and ultrasonic inspection at acceptance grades 2-3, is mandatory.

Casting Process Analysis and Design

Selection of Pouring Position

The choice of pouring position is fundamental, impacting everything from mold design to final quality. For cylinder-type ductile iron castings, two primary orientations are considered: pouring with the horizontal joint (mid-plane) facing down or facing up.

Mid-plane Down Orientation: In this scheme, metal enters the mold cavity at the joint face. While this can distribute initial oxide dross onto non-critical surfaces, it often leads to extensive cleaning and grinding, risking wall thickness violation if overdone. The cores can be supported within the mold’s footprint, allowing for a relatively compact flask size and lower sand consumption. However, assembly is tricky: cores must be placed before the cope, making wall thickness control and inspection difficult. Furthermore, cores are susceptible to buoyant forces during pouring, potentially causing dimensional shifts.

Mid-plane Up Orientation: Here, metal is introduced from the bottom, near the inlet flange and end walls. The initial dross rises and is trapped on the upper surfaces of internal ribs and the joint face—all machined areas where it is completely removed during finishing, eliminating manual grinding. This necessitates a suspended core design with core prints extending beyond the part footprint, requiring a larger flask and more sand. The assembly sequence is reversed and more robust: the drag and cope are assembled first, followed by core placement. This allows for precise measurement and control of wall thicknesses. Crucially, the weight of the cope mold helps counteract core buoyancy during pouring.

A comparative analysis clearly favors the mid-plane up orientation for this application. Although it consumes more sand, the benefits in operational simplicity, dimensional control, and final quality assurance for these high-integrity ductile iron castings are decisive.

Gating System Design

To minimize oxidation and promote tranquil mold filling, a bottom-gating system was adopted. Analyzing the casting geometry, ingates were strategically located at the bottom of the central inlet flange and at the two end wall arcs. This created three relatively independent gating systems, each fed by its own downsprue. The system was designed as open, with the choke at the downsprue. The typical area ratios for the systems were:
$$ \Sigma S_{\text{sprue}} : \Sigma S_{\text{runner}} : \Sigma S_{\text{ingate}} = 1 : 1.2\text{–}1.5 : 3.0\text{–}5.0 $$
A significant height difference exists between the central and end feed points. To prevent turbulent meeting of metal streams and potential backflow, a calculated delay was introduced in opening the central gating system. This technique ensured the metal levels from the bottom and sides rose and met smoothly within the mold cavity.

Core Assembly Design

The core design addressed two major challenges inherent in the complex geometry of these ductile iron castings.

1. Volute Passage and Draft Angles: The core for the internal volute steam path was split. The section inside the inlet pipe was made separately from the main passage core. The external part of the inlet pipe core was parted along its flow centerline for easy pattern withdrawal. During molding, the internal inlet core was set first, followed by the external inlet core, and finally the main passage core, resolving draft and interference issues.

2. Internal Diaphragm Cavities: The narrow, angled spaces between internal diaphragms precluded the use of a single, large core. The innovative solution was a laminated core assembly. The internal cavity was partitioned along the edges of the diaphragms into seven segments. Each segment, combined with the adjacent diaphragm walls, formed an individual core. These were supported by an overhead suspension frame. Assembly proceeded by placing the volute core first, then sequentially adding the laminated cores from the center outward. This approach ensured core strength, allowed for individual core production, and enabled precise wall thickness verification for every section before closing the mold.

Chill Design

Ductile iron solidifies in a mushy mode and has poor weldability, making the prevention of shrinkage porosity through controlled cooling paramount. A zone-based analysis was conducted:

  • Main Thin Walls: These sections, subdivided by flanges and ribs, cool rapidly and can achieve directional solidification, requiring no chills.
  • Thick Horizontal Flange (210 mm): With a modulus >3 cm, simultaneous solidification is impossible. However, under the right conditions—carbon equivalent (CE) > 4.5% and high mold rigidity (sand compression strength > 3 MPa)—the graphite expansion during eutectic solidification can provide adequate self-feeding to counteract shrinkage, negating the need for chills. The self-feeding capacity can be assessed by comparing the volume of graphite expansion to the volume of liquid contraction. A simplified condition for soundness in a restrained section is:
    $$ V_{graphite} \cdot \rho_{graphite} \cdot \alpha \geq V_{casting} \cdot \beta \cdot \Delta T \cdot \gamma $$
    Where $V_{graphite}$ is the volume of graphite precipitated, $\rho_{graphite}$ is its density, $\alpha$ is an expansion efficiency factor (dependent on mold rigidity), $V_{casting}$ is the casting volume, $\beta$ is the liquid contraction coefficient, $\Delta T$ is the temperature drop during liquid contraction, and $\gamma$ is a geometrical factor. For flange sections, high CE and rigid molds ensure this inequality holds.
  • Internal Diaphragm Machined Faces: These areas cannot solidify directionally nor rely fully on self-feeding due to their geometry and connection to thinner sections. Therefore, chills were essential here. The chill thickness ($t_{chill}$) was designed relative to the local casting thickness ($t_{casting}$):
    $$ t_{chill} = (0.8 \text{ to } 1.2) \times t_{casting} $$

Riser (Feeder) Design

In principle, a well-designed ductile iron casting that achieves effective self-feeding does not require conventional risers for liquid feeding. However, given the structural complexity and potential for minor core shift or local thickness variation, a safety margin of liquid metal is prudent during the initial liquid contraction phase. Therefore, 6 to 8 small risers were placed on the cope, holding approximately 2.5% of the total poured weight. These were connected to the casting via thin, constricted necks. This design serves a dual purpose: 1) It provides a limited liquid feed source during the early liquid contraction stage, and 2) The necks freeze rapidly, isolating the casting from the atmosphere and the large thermal mass of the riser shortly after filling, thereby creating a closed system that efficiently utilizes the internal graphite expansion pressure for feeding. The risers also serve as excellent vents during pouring.

Solidification Simulation and Analysis

Following the initial process design, a full 3D model was created for simulation using MAGMAsoft. The goals were to visualize filling patterns for turbulence and to predict shrinkage porosity formation using criteria such as the Niyama criterion ($G/\sqrt{\dot{R}}$), where $G$ is the thermal gradient and $\dot{R}$ is the cooling rate. Regions where this value falls below a critical threshold indicate a high risk for microporosity. The simulation process involved iteratively analyzing temperature fields and solidification sequences, leading to optimization of chill placement, riser size/location, and gating details before any tooling was committed. This virtual prototyping is indispensable for first-time-right production of complex ductile iron castings.

Production Trials and Results

Melting, Pouring, and Heat Treatment

Iron was melted in a medium-frequency induction furnace. The target chemical composition, crucial for achieving the required graphite structure and matrix, is detailed in Table 1. The ladle treatment involved a sandwich method for nodularization and primary inoculation. A transfer ladle was used for a secondary inoculation stream during pouring into a holding furnace. After a 2-minute dwell for slag separation, the metal was poured at a carefully controlled temperature of 1,340–1,360 °C. The pouring time was maintained between 120 and 300 seconds; exceeding this risks cold laps due to excessive heat loss.

Table 1: Chemical Composition Requirements and Results (Mass %)
Element Pre-Treatment Target Post-Treatment Result
Carbon (C) 3.5 – 3.7 3.6 – 3.8
Silicon (Si) 1.4 – 1.8 2.2 – 2.4
Manganese (Mn) ≤ 0.20 ≤ 0.20
Sulfur (S) ≤ 0.020 ≤ 0.020
Phosphorus (P) ≤ 0.040 ≤ 0.040
Magnesium (Mg) – 0.035 – 0.050

Castings were shaken out after cooling below 300°C. Following initial cleaning, a stress-relief annealing treatment was performed to eliminate residual casting stresses, preventing potential distortion during subsequent machining which could compromise sealing and assembly.

Metallographic Structure and Mechanical Properties

Test coupons attached to the casting were evaluated. The microstructure, consisting of >95% ferrite with well-formed, isolated graphite nodules in a matrix free of carbides, is the foundation for the high ductility of these ductile iron castings. The specific results are summarized in Table 2.

Table 2: Metallographic Inspection Results from Attached Test Coupons
Inspection Item Standard (QT400-18A) Measured Result
Nodularity Grade 1-3 2
Nodule Size Grade 5-7 6
Ferrite Content ≥ 95% > 95%
Pearlite Content ≤ 5% < 5%
Carbide Content ≤ 1% 0%
Matrix Structure Ferrite + Graphite Ferrite + Graphite

The mechanical properties, the ultimate validation of the process, were tested and comfortably exceeded the specification requirements for QT400-18A, as shown in Table 3. The high elongation and impact values are direct results of the sound, ferritic microstructure achieved in these large-section ductile iron castings.

Table 3: Mechanical Property Test Results
Property Standard (QT400-18A) Measured Result
Yield Strength (Rp0.2) ≥ 240 MPa 267 MPa
Tensile Strength (Rm) ≥ 370 MPa 392 MPa
Elongation (A) ≥ 12 % 25.5 %
Hardness (HBW) 130 – 180 138
Charpy Impact (Room Temp) Avg. ≥ 12 J, Single ≥ 9 J 18 J, 19 J, 19 J

Finally, 100% non-destructive testing (Magnetic Particle and Ultrasonic) was conducted on the rough casting. The inspection results confirmed the absence of significant defects, with all indications well within the specified acceptance levels (Grade 2-3), validating the effectiveness of the entire manufacturing process for these critical ductile iron castings.

Conclusions

1. Through systematic analysis, an optimal casting process was established for large thermal power low-pressure inner cylinders. Key decisions included adopting a mid-plane up, bottom-gated pouring position; designing a laminated core assembly for complex internal passages; implementing strategic chills on isolated hot spots; and using small safety risers. This process was validated and refined through MAGMA numerical simulation, confirming its capability to produce sound ductile iron castings.

2. Rigorous control during melting, treatment, pouring, and heat treatment, aligned with the designed process, yielded castings that fully met all technical specifications. The metallographic structure showed excellent nodularity and a ferritic matrix, directly translating into mechanical properties that surpassed the requirements of QT400-18A, including exceptional elongation and impact toughness. Successful NDT results further confirmed internal soundness.

3. The successful series production of multiple units of this component type demonstrates conclusively that monolithic ductile iron castings are a technically superior and economically viable alternative to traditional fabricated steel plate assemblies for large power generation components. The casting process offers inherent advantages in geometric integrity, production efficiency, and cost, paving the way for wider adoption in the energy sector and beyond.

Scroll to Top