In my work on automotive transmission components, I have found that the gearshift fork is one of the most demanding parts in terms of both mechanical performance and dimensional stability. This part is located at the lower end of the gearshift handle and is connected to the handle. During driving, the fork moves the synchronizer sleeve and changes the position of the gears inside the transmission, thereby changing the input-to-output speed ratio and enabling gear shifting. Because the gear rotates at high speed while the fork itself does not rotate, any insufficient mechanical strength or excessive wear can prevent the gear from engaging fully, cause the gear to jump out, or even fracture the fork. Therefore, the gearshift fork has very high quality requirements, and the design and production of ductile iron castings for this application present significant difficulties.
This article describes a casting process method for an automotive ductile iron gearshift fork. The original process could place only two castings horizontally in one mold. Without changing the molding equipment, I used vertical placement and a single feeder per casting to arrange three castings in one mold. I designed a casting process that satisfies all quality requirements. Through simulation analysis and practical verification, the produced castings meet all requirements of the customer-specified standard, and the process is now ready for mass production.
The material is ductile iron, grade EN-GJS-600-3, which is equivalent to QT600-3 in GB/T 1348—2009. The single casting weight is 3.05 kg, the maximum length is 365 mm, the average width is 16 mm, the main wall thickness is 33 mm, and the thickest section is 50 mm. The casting has an arched, long strip shape. The production line uses a DISA 231 vertical parting flaskless shoot-squeeze molding machine. The pattern plate size is 650 mm × 535 mm. Melting is performed in a medium-frequency induction furnace, and the metal is spheroidized by the wire-feeding method.

Main Technical Requirements
The technical requirements for the gearshift fork are strict and cover microstructure, mechanical properties, chemical composition, internal soundness, surface roughness, and freedom from distortion. Table 1 summarizes the main requirements. These requirements are typical for high-performance ductile iron castings used in automotive transmissions.
| Category | Requirement |
|---|---|
| Graphite nodularity | ≥ 85% |
| Cementite volume fraction | < 1% |
| Matrix structure | Pearlite + ferrite, pearlite ≥ 50% |
| Graphite size | Grade 5 to 8 |
| Tensile strength | ≥ 600 MPa |
| Yield strength | ≥ 380 MPa |
| Elongation | ≥ 3% |
| Brinell hardness | 200 to 250 HBW |
| Silicon content | < 2.80% |
| Titanium content | < 0.03% |
| Internal defects | No cracks, slag holes, or gas pores; ASTM E689 level ≤ 2 |
| Surface roughness | Ra < 100 μm; no slag holes or sand holes affecting assembly or appearance |
| Distortion | No warping or twisting that affects assembly or appearance |
For ductile iron castings, the combination of high tensile strength, moderate elongation, and a pearlite content of at least 50% requires careful control of carbon equivalent, silicon, manganese, copper, and residual magnesium. The carbon equivalent is often expressed as:
$$ CE = C + \frac{Si}{3} + \frac{P}{3} $$
In my process, the carbon equivalent is maintained in a range that promotes graphitization while avoiding excessive shrinkage. The silicon content must remain below 2.80% because higher silicon increases ferrite formation and reduces pearlite. Titanium must remain below 0.03% because titanium promotes the formation of titanium carbides and can deteriorate machinability and impact toughness. The residual magnesium must be high enough to achieve a nodularity of at least 85% but not so high that it causes dross, slag, or shrinkage porosity.
Original Process and Its Limitations
Because the casting length is large, and because adding the two feeding risers at both ends increases the total length, the pattern dimensions already reach the upper limit of the molding chamber. Based on previous design experience, I initially selected a horizontal layout with only two castings per mold. In this original process, the metal utilization rate was only 36%. The top edge of the fork leg, within about 2 mm, contained 8% to 12% free cementite. The position of the free cementite on the casting and the microstructure are shown in the original figures, but the key issue is that this hard, brittle phase degrades machinability and fatigue resistance.
Because the mold produced by the vertical molding machine has lower compactness at the lowest part of the cavity, the bottom of the casting suffered from severe mechanical sand burn-on. Due to the structure of the casting itself, shrinkage during solidification in green sand easily caused the head and tail ends to warp relative to the middle. In addition, the metal had a large height drop from the pouring cup to the casting, causing turbulent flow in the gating system. This led to severe slag holes and sand holes near the riser neck at the lower part of the casting, requiring rejection.
The metal utilization rate can be defined as:
$$ \eta = \frac{m_{\text{castings}}}{m_{\text{poured}}} \times 100\% $$
For the original two-casting layout, if the total poured metal mass was about 16.9 kg and the casting mass was 3.05 kg each, then:
$$ \eta_{\text{original}} = \frac{2 \times 3.05}{16.9} \times 100\% \approx 36\% $$
This low efficiency increased melting energy, sand consumption, and the amount of returned metal. It also increased the risk of defects because a large volume of metal had to be poured through a long gating system.
Redesigned Process: Vertical Arrangement with Three Castings per Mold
After calculation, CAE simulation, and review, I modified the original process. The main change was to convert the horizontal two-casting layout into a vertical three-casting layout. I achieved this without changing the molding equipment. Each casting uses only one feeder, and the three castings are arranged vertically in the mold. This arrangement reduces the projected area required per casting and allows better use of the pattern plate.
To solve the distortion problem and to reduce internal porosity in some fork legs, I added an anti-deformation tie bar between the upper and lower fork legs of each pattern. The tie bar has a thickness of 4 mm and a width of 20 mm. The first casting on the left uses one tie bar connecting its upper and lower fork legs. The second and third castings share one tie bar arranged in a cross shape. The four ends of this cross-shaped tie bar connect to the upper and lower fork legs of the second casting and the upper and lower fork legs of the third casting. To facilitate removal from the casting without tearing metal and to minimize residual grinding, the connection between each tie bar end and the fork leg has a thickness equal to half of the tie bar body thickness, while the width remains unchanged.
The new process has several important advantages. The tie bars create conditions that favor directional solidification and shrinkage of the upper and lower ends of the casting. During solidification and contraction, the tie bars effectively decompose the internal stress that would otherwise cause twisting. Because the tie bars are thin and plate-like, they solidify before the casting. Once solidified, they prevent the upper and lower fork legs from moving toward the middle or deforming vertically. They act as supports and tension members, so the casting does not twist during solid contraction.
As the metal temperature continuously decreases after pouring, the tie bars remain much cooler than the casting because of their thinner wall thickness. They transfer heat away from the local casting regions, accelerating solidification and acting as chills. This helps prevent internal porosity in the fork leg regions. Because the tie bars are used, the produced castings do not require secondary heating or special fixtures for high-temperature correction of twisting. This eliminates electric furnace heating and correction, saving electrical energy and labor cost.
The tie bars also allow the first incoming floating sand and supercooled metal to enter the tie bar cavities, further reducing sand holes and slag holes on the casting surface and improving surface quality. After shakeout, shot blasting, and cooling to room temperature, the tie bars can be removed together with the runners and risers by a hydraulic separator. They then enter the returned scrap circulation system without additional separate handling.
Most importantly, the use of tie bars reduces the number of risers. The original process required six risers per mold for two castings. The new process requires only three risers for three castings, meaning each casting has only one superheated riser. The metal utilization rate increases to 54%, which is 1.5 times that of the original two-casting process. Production efficiency also increases to 1.5 times the original.
The improvement in metal utilization can be expressed as:
$$ \eta_{\text{new}} = \frac{3 \times 3.05}{16.9} \times 100\% \approx 54\% $$
Table 2 compares the original and improved processes.
| Item | Original process | Improved process |
|---|---|---|
| Castings per mold | 2 | 3 |
| Layout | Horizontal | Vertical |
| Risers per mold | 6 | 3 |
| Risers per casting | 3 | 1 |
| Metal utilization | 36% | 54% |
| Relative production efficiency | 1.0 | 1.5 |
| Anti-deformation tie bars | None | Used |
| Free cementite at fork leg edge | 8% to 12% | Not observed |
| Sand burn-on at bottom | Severe | Controlled |
| Warping and twisting | Significant | Eliminated |
CAE Simulation with MAGMA
I used MAGMA simulation software to analyze the filling process of the designed casting process. In the DISA sand mold casting module, I imported the 3D graphics converted to STL format and set the attributes, boundary conditions, and heat transfer coefficients. I meshed all components and generated more than 21 million cells. I input the basic conditions of the DISA 231 molding line, the mold thickness, and the relative positions of all components. Then I imported the chemical composition, pouring temperature, pouring time, and shakeout temperature. After checking, I started the numerical simulation.
The pouring temperature field, solidification rate, solidification time, and porosity distribution were simulated. The numerical simulation results showed that the newly designed process meets the requirements of the casting production process. After the molds, core boxes, and core-setting frames were manufactured, I performed actual debugging and verification.
The solidification time can be estimated by Chvorinov’s rule:
$$ t_s = B \left(\frac{V}{A}\right)^n $$
where \(t_s\) is the solidification time, \(V\) is the volume, \(A\) is the surface area, \(B\) is a mold constant, and \(n\) is an exponent typically between 1.5 and 2.0. The modulus of the casting is:
$$ M = \frac{V}{A} $$
For a sound casting, the modulus of the riser should be greater than that of the casting section it feeds:
$$ M_r \geq 1.2 M_c $$
In the new design, the single riser per casting is sized to satisfy this condition. The anti-deformation tie bars act as chills, reducing the local modulus and promoting directional solidification toward the riser. Table 3 lists the key simulation parameters.
| Parameter | Value |
|---|---|
| Simulation software | MAGMA |
| Molding module | DISA sand mold |
| Number of cells | > 21 million |
| Pouring temperature | 1 370 to 1 420 °C |
| Mold thickness | As per DISA 231 |
| Shakeout temperature | Produced according to process |
| Initial metal composition | As designed for EN-GJS-600-3 |
The simulation showed that the vertical three-casting layout with one riser per casting produced a smooth filling pattern. The temperature field indicated that the last solidifying region was located in the riser, not in the casting. The solidification rate and solidification time results confirmed that the fork legs solidified before the riser neck, allowing the riser to feed the casting effectively. The porosity prediction showed no unacceptable shrinkage defects. These results gave confidence that the process would meet the ASTM E689 level ≤ 2 requirement for internal defects.
Melting and Metal Treatment
I used a 4 t medium-frequency induction furnace for melting. The charge consisted of returned gating and riser systems, rejected ductile iron castings, Q10 pig iron, and low-chromium, low-manganese, rust-free bundled stamped steel scrap. To ensure complete dissolution and absorption of the carburizer, I used a low-sulfur, high-absorption graphite carburizer. The carburizer was charged together with the scrap, pig iron, and returned material. The charge formula was 50% steel scrap + 40% returned material + 10% pig iron + carburizer. Table 4 lists the melting process parameters.
| Parameter | Value |
|---|---|
| Sampling temperature | 1 430 to 1 480 °C |
| Holding time | 3 to 4 min |
| Holding temperature | 1 530 to 1 540 °C |
| Tap temperature | 1 510 to 1 520 °C |
| Tap mass | 596 to 604 kg |
I used a cored spheroidizing wire as the spheroidizing agent. The rare earth content was 10.0% to 13.0%, and the magnesium content was 7.5% to 8.5%. Before spheroidization, the sulfur content in the iron was controlled below 0.025%. To ensure the necessary residual magnesium after spheroidization, the core powder addition of the cored wire was controlled at about 0.60%. During tapping, I ensured consistency in the tap mass, tap temperature, and iron turnover time. To prevent shrinkage porosity caused by excessive residual magnesium, I strictly controlled the spheroidizing temperature between 1 460 and 1 480 °C and the reaction time between 45 and 65 s. Table 5 lists the wire-feeding spheroidization parameters.
| Parameter | Value |
|---|---|
| Wire length | 13 ± 0.15 m |
| Temperature before wire feeding | 1 455 to 1 490 °C |
| Wire feeding speed | 18 ± 0.2 m/min |
| Reaction time | 45 to 65 s |
| Temperature after wire feeding | 1 430 to 1 445 °C |
Inoculation was performed in three stages. Before treatment, the silicon content of the base iron was controlled at 1.30% to 1.40%. During tapping, the first inoculation was performed with 0.30% of 75SiFe inoculant. After wire-feeding spheroidization, while pouring the metal into the pouring ladle, the second inoculation was performed by the stream method with 0.30% of 75SiFe inoculant. During pouring, the third inoculation was performed by instantaneous stream inoculation with 0.10% of a 75% Si, 4% Ba inoculant. The pouring temperature was controlled at 1 370 to 1 420 °C. During the wire-feeding spheroidization reaction, the ladle cover was kept tightly closed to avoid and reduce splashing of metal containing magnesium and rare earth elements, which could cause poor spheroidization or spheroidization decay. This also helped the workshop environmental equipment to extract and remove dust, avoiding environmental pollution.
Chemical Composition
According to the designed chemical composition requirements, I sampled the test-produced castings and analyzed the chemical composition using a PDA5500IV optical emission spectrometer. Table 6 shows the actual chemical composition test results. The silicon content remains below 2.80%, and the titanium content remains below 0.03%, satisfying the customer’s special requirements. The carbon content is around 3.75% to 3.79%, the manganese content is about 0.46% to 0.49%, and the copper content is about 0.43% to 0.47%. The residual magnesium is 0.030% to 0.033%, and the residual rare earth elements are low. These values are appropriate for producing high-strength ductile iron castings with a predominantly pearlitic matrix.
| Sample | C | Si | Mn | P | S | Cu | Ni | Cr | V | Ti | Al | Residual Mg | Residual La | Residual Ce |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| 1 | 3.751 | 2.451 | 0.490 | 0.027 | 0.011 | 0.431 | 0.010 | 0.016 | 0.011 | 0.020 | 0.010 | 0.032 | 0.007 | 0.010 |
| 2 | 3.760 | 2.463 | 0.483 | 0.028 | 0.008 | 0.470 | 0.013 | 0.020 | 0.013 | 0.021 | 0.012 | 0.030 | 0.006 | 0.010 |
| 3 | 3.770 | 2.454 | 0.460 | 0.026 | 0.010 | 0.469 | 0.012 | 0.018 | 0.010 | 0.017 | 0.011 | 0.031 | 0.005 | 0.014 |
| 4 | 3.790 | 2.421 | 0.456 | 0.025 | 0.009 | 0.437 | 0.010 | 0.017 | 0.015 | 0.023 | 0.012 | 0.030 | 0.007 | 0.013 |
| 5 | 3.763 | 2.461 | 0.480 | 0.029 | 0.012 | 0.450 | 0.013 | 0.021 | 0.014 | 0.022 | 0.010 | 0.033 | 0.006 | 0.015 |
The carbon equivalent for the average composition can be calculated as:
$$ CE = 3.764 + \frac{2.450}{3} + \frac{0.027}{3} \approx 4.59\% $$
This carbon equivalent is near the eutectic range, which favors good castability and feeding. However, because the silicon content is kept below 2.80%, the risk of excessive ferrite is reduced, and the pearlite content can be maintained above 50%. The low titanium content avoids titanium carbide formation, which is important for machinability and fatigue resistance in ductile iron castings.
Microstructure
I used a BM4XAⅡ metallographic microscope and followed ASTM 1245—2003 to examine the microstructure of samples taken from the casting body. The graphite nodularity was 90%. The matrix structure was mainly fine ferrite with pearlite ≥ 50%, and no carbides were observed. In addition, I used an online sound velocity measuring instrument to inspect the nodularity of the castings. The nodularity of the castings was between 90% and 95%. The nodularity can be defined as:
$$ SG = \frac{N_{\text{spheroidal}}}{N_{\text{total}}} \times 100\% $$
where \(N_{\text{spheroidal}}\) is the number of spheroidal graphite particles and \(N_{\text{total}}\) is the total number of graphite particles. The sound velocity method is based on the principle that the acoustic velocity through a ductile iron casting depends on the shape of the graphite. For the gearshift fork, the main wall thickness is about 33 mm, and the flat area measured by the sound velocity instrument is 16 mm thick. Through a large number of comparative tests, I set the sound velocity range to 5 350 to 5 500 m/s. If the measured sound velocity is within this range, the nodularity of the casting is judged to be between 90% and 95%. The sound velocity measurement can also indirectly indicate whether the internal structure of the measured area is dense and free of defects. If the sound velocity is too low, it indicates the presence of hole-type defects inside the casting.
The pearlite content can be estimated by area fraction:
$$ P = \frac{A_{\text{pearlite}}}{A_{\text{total}}} \times 100\% $$
For the tested samples, \(P \geq 50\%\), which satisfies the requirement. The graphite size was within grade 5 to 8. The absence of free cementite is particularly important because free cementite at the fork leg edge was a defect in the original process. The improved process, with its vertical arrangement and anti-deformation tie bars, provides a better thermal balance and reduces the formation of chilled structures.
Mechanical Properties
I sampled the test-produced castings and used an XYA105C universal tensile testing machine to test the mechanical properties of machined specimens. I used an HB-3000B Brinell hardness tester to measure the hardness of the casting body. Table 7 shows the mechanical properties and Brinell hardness results. The tensile strength ranges from 665 to 734 MPa, the yield strength ranges from 403 to 441 MPa, the elongation ranges from 5.1% to 7.6%, and the Brinell hardness ranges from 203 to 230 HBW. All values meet the requirements of tensile strength ≥ 600 MPa, yield strength ≥ 380 MPa, elongation ≥ 3%, and hardness 200 to 250 HBW.
| Sample | Tensile strength (MPa) | Yield strength (MPa) | Elongation (%) | Brinell hardness (HBW) |
|---|---|---|---|---|
| 1 | 675 | 413 | 6.3 | 220 |
| 2 | 734 | 441 | 5.3 | 230 |
| 3 | 733 | 420 | 6.6 | 222 |
| 4 | 710 | 403 | 7.6 | 203 |
| 5 | 665 | 406 | 5.1 | 218 |
The relationship between Brinell hardness and tensile strength in pearlitic ductile iron castings can be approximated by:
$$ HBW \approx \frac{UTS}{3.2 \text{ to } 3.5} $$
For example, with a tensile strength of 734 MPa and a hardness of 230 HBW, the ratio is about 3.19, which is consistent with a high-strength ductile iron casting. The mechanical property results confirm that the alloying and cooling conditions produce a pearlite content above 50% and a fine graphite structure.
Prohibited Substances
I tested samples taken from the casting body using a spectrophotometer supplemented by chemical analysis. Table 8 shows that the contents of prohibited substances meet the requirements. The cadmium content is 0.007%, hexavalent chromium is below 0.038%, lead is 0.019%, and mercury is below 0.021%. I also created a material database for the automotive gearshift fork in the IMDS system, and the IMDS report has been approved in writing by the customer.
| Item | Specified value | Measured value |
|---|---|---|
| Cadmium | < 0.01 | 0.007 |
| Hexavalent chromium | < 0.10 | < 0.038 |
| Lead | < 0.10 | 0.019 |
| Mercury | < 0.10 | < 0.021 |
Appearance and Internal Quality
I used a through-type hanging shot blasting machine for surface cleaning. I added alloy steel shot with a grain size of 0.8 to 1.2 mm, at 50% of the total shot weight, and cut-wire steel shot with a grain size of 0.7 to 1.0 mm, also at 50% of the total shot weight. After shot blasting, I performed 100% visual inspection on every batch. Compared with a roughness comparator, the average surface roughness of the castings reached 35 to 65 μm, satisfying the customer requirement of Ra < 100 μm. No slag holes or sand holes affecting assembly or appearance were found.
I also used a sound velocity instrument for nodularity inspection. The sound velocity range was 5 350 to 5 500 m/s, corresponding to a nodularity of 90% to 95%. The instrument also helped identify internal density variations. For X-ray inspection, I used a through-type X-ray inspection device. The results showed that all internal defects met ASTM E689 level ≤ 2. No shrinkage porosity was found in the castings. For magnetic particle inspection, I used a through-type magnetic particle inspection machine to inspect all positions of the casting. This method can clearly identify both hot cracks formed during solidification and cold cracks formed after solidification due to stress. The inspection results showed that no cracks or other crack-like defects were found in any casting.
The combination of these non-destructive tests provides a high level of confidence in the internal quality of the ductile iron castings. Table 9 summarizes the inspection methods and acceptance criteria.
| Inspection method | Purpose | Acceptance criterion |
|---|---|---|
| Visual inspection | Surface defects | No slag holes or sand holes affecting assembly or appearance |
| Roughness comparator | Surface roughness | Ra < 100 μm |
| Sound velocity | Nodularity and internal density | 5 350 to 5 500 m/s; nodularity 90% to 95% |
| X-ray | Internal defects | ASTM E689 level ≤ 2 |
| Magnetic particle | Cracks | No cracks or crack-like defects |
Discussion
The production of high-quality ductile iron castings for gearshift forks requires an integrated approach that considers alloy design, melting, spheroidization, inoculation, gating, feeding, and mold layout. In my work, the most important process change was the transition from a horizontal two-casting layout to a vertical three-casting layout with one riser per casting and anti-deformation tie bars. This change increased the metal utilization rate from 36% to 54% and increased production efficiency by 1.5 times. It also eliminated free cementite at the fork leg edge, reduced sand burn-on at the bottom of the mold, prevented warping and twisting, and reduced slag holes and sand holes near the riser neck.
The thermal conditions in the vertical mold are more uniform than in the horizontal mold. In the vertical arrangement, the three castings occupy a smaller projected area, and the mold filling pattern is more balanced. The anti-deformation tie bars act as chills and structural supports. Because they are thin, they solidify early and acquire a lower temperature than the casting. This promotes directional solidification from the fork legs toward the riser. The modulus of the tie bar is small, so it does not act as a feeding path but rather as a cooling fin. The riser modulus is designed to be at least 1.2 times the modulus of the casting section, ensuring that the riser remains liquid until the casting has solidified.
The chemical composition is also critical. The carbon equivalent of about 4.59% is close to the eutectic point, which improves fluidity and feeding. The silicon content is kept below 2.80% to avoid excessive ferrite and to maintain the required pearlite content. The manganese content of about 0.46% to 0.49% helps stabilize pearlite. Copper at about 0.43% to 0.47% also promotes pearlite and increases hardenability. The residual magnesium of 0.030% to 0.033% is sufficient for nodularity above 90% without causing excessive dross or shrinkage. The titanium content is below 0.03%, preventing titanium carbide formation. The low sulfur and phosphorus contents also contribute to good mechanical properties.
The three-stage inoculation is important for obtaining a uniform microstructure and avoiding chill. The first inoculation during tapping provides nucleation sites. The second inoculation during transfer to the pouring ladle helps counteract spheroidization decay. The third inoculation during pouring provides instantaneous nucleation in the mold. This combination ensures that the graphite nodules are small and uniformly distributed, with a nodularity of 90% to 95%. The absence of free cementite is a direct result of the improved inoculation and the thermal effects of the anti-deformation tie bars.
The mechanical properties exceed the minimum requirements. The tensile strength of 665 to 734 MPa is well above 600 MPa. The yield strength of 403 to 441 MPa is above 380 MPa. The elongation of 5.1% to 7.6% is above 3%. The Brinell hardness of 203 to 230 HBW is within the specified range of 200 to 250 HBW. These properties are consistent with a pearlite content of at least 50%, a nodularity of at least 85%, and a fine graphite size. The X-ray and magnetic particle inspections confirm that the internal quality meets the customer’s requirements. The surface roughness of 35 to 65 μm is well below the maximum of 100 μm. The absence of warping and twisting ensures that the gearshift fork can be assembled without additional correction.
The economic benefits of the improved process are significant. The metal utilization rate increased from 36% to 54%. This reduces melting energy, raw material consumption, and returned scrap. The production efficiency increased by 1.5 times, which reduces labor cost per casting. The elimination of secondary heating and correction saves electrical energy and labor. The reduction in risers from six to three per mold reduces the amount of metal that must be cut off and returned. The anti-deformation tie bars are removed together with the runners and risers, so no additional handling is required. The process is therefore both technically and economically advantageous for ductile iron castings.
Looking forward, I plan to further improve the process. Without changing the existing molding equipment, I plan to use the vertical three-casting layout but add a resin-coated sand partition core between the castings. This would allow the three-casting layout to become a six-casting layout. The resin-coated sand partition core would increase the mold strength, effectively preventing distortion. It would also allow the anti-deformation tie bars connecting the upper and lower fork legs to be removed, reducing metal consumption and further improving metal utilization. Calculations indicate that using the resin-coated sand partition core could increase the metal utilization rate to at least 66%. If necessary, I will explore additional methods to further improve the production feasibility of ductile iron castings for gearshift forks that meet customer requirements.
Conclusions
1. The simulation analysis and casting body inspection results show that the optimized casting process produces gearshift fork castings whose mechanical properties and internal quality meet all customer requirements. Through verification and reliability analysis of multiple batches over several months, the process is confirmed to meet the initial design requirements for the ductile iron castings.
2. The casting process system was changed from the original two-casting layout to a three-casting layout. After two improvements, the final metal utilization rate reached 54%. The anti-deformation tie bars, the vertical arrangement, and the single riser per casting were the key features that made this possible.
3. The chemical composition, microstructure, mechanical properties, prohibited substance content, surface roughness, and internal defect levels all meet the customer’s specifications. The nodularity is 90% to 95%, the pearlite content is at least 50%, the tensile strength is 665 to 734 MPa, the yield strength is 403 to 441 MPa, the elongation is 5.1% to 7.6%, and the Brinell hardness is 203 to 230 HBW.
4. Future work will focus on using a resin-coated sand partition core to convert the three-casting layout into a six-casting layout, removing the anti-deformation tie bars, and increasing the metal utilization rate to at least 66%. This will further reduce cost and improve the competitiveness of the ductile iron castings for automotive gearshift forks.
In summary, the casting process I developed demonstrates that high-quality ductile iron castings for gearshift forks can be produced efficiently on a vertical parting flaskless molding line. The combination of vertical placement, one riser per casting, anti-deformation tie bars, controlled melting and spheroidization, three-stage inoculation, and rigorous inspection ensures that the castings meet all specified requirements. The process is now ready for mass production, and the planned future improvements will further increase metal utilization and reduce manufacturing cost.