Local Squeeze-Assisted HPDC for Reducing Casting Defects in Engine Brackets

I conducted this study to reduce casting defects in an automotive engine bracket produced by high-pressure die casting (HPDC). The bracket is a safety-critical connection component between the engine and the subframe. Because of lightweight design requirements, the bracket has a complex geometry, non-uniform wall thickness, and large height differences between the parting surfaces. These features make it difficult to vent the die cavity and to transmit intensification pressure to the last-filled regions. As a result, casting defects, especially gas porosity and shrinkage porosity, appear near the remote bearing hole. These casting defects reduce the local density, strength, and fatigue performance of the bracket. My objective was to combine CAE simulation, process optimization, and local squeeze technology to reduce casting defects and to establish an efficient production method for HPDC engine brackets.

I used a systematic approach that included theoretical analysis, numerical simulation with commercial casting software, Taguchi-based process optimization, and experimental validation by X-ray inspection and sectioning. I first analyzed the mechanisms of gas porosity and shrinkage porosity in HPDC. I then simulated the filling and solidification processes to predict the locations and types of casting defects. After that, I optimized the conventional HPDC parameters, including intensification pressure, high-speed velocity, and high-speed interval. Because the optimized conventional process could not reduce the local porosity to an acceptable level, I designed and implemented a local squeeze system. I studied the effects of squeeze delay time, squeeze depth, and squeeze duration on casting defects. The final results showed that local squeeze-assisted HPDC can reduce the maximum pore diameter to 0.46 mm and the local porosity to 0.6%, which meets the relevant acceptance level.

1. Background and Motivation

The automotive industry is under continuous pressure to reduce vehicle weight, improve fuel efficiency, and lower emissions. Aluminum alloys are attractive because of their low density and high specific strength. HPDC is one of the most widely used production methods for aluminum automotive components because it can produce thin-walled, complex, and near-net-shape parts with good dimensional accuracy. However, HPDC also has inherent disadvantages. During filling, the metal melt can entrap air, and during solidification, volume contraction and uneven cooling can create casting defects. Gas porosity and shrinkage porosity are among the most common and harmful casting defects in HPDC parts.

In the engine bracket studied here, the remote bearing hole is located above the main parting plane. This geometry prevents the installation of an effective vent or overflow at that location. The melt reaches this region last, and the intensification pressure cannot be transmitted effectively through the already solidified gate. Consequently, casting defects accumulate around the bearing hole. The local porosity can reach 9.0% before optimization, and the maximum pore diameter can reach 3.2 mm. Such casting defects are unacceptable for a load-bearing engine bracket.

I aimed to answer three questions. First, what are the main causes of casting defects in this bracket? Second, can conventional process optimization reduce these casting defects to an acceptable level? Third, if conventional optimization is insufficient, how can local squeeze technology be designed and controlled to reduce casting defects further? My work provides a complete workflow that links simulation, mold design, process optimization, and local squeeze assistance.

2. Theoretical Basis of HPDC and Casting Defects

HPDC is a precision casting process in which molten metal is injected into a die cavity at high speed and solidified under high pressure. The combination of high pressure and high speed distinguishes HPDC from gravity casting and low-pressure casting. The flow behavior of the melt inside the die cavity controls the final distribution of casting defects. Classical filling theories describe different filling patterns, but in practice the actual filling behavior depends on gate geometry, die temperature, melt temperature, injection velocity, and the pressure profile.

I considered the melt as an incompressible Newtonian fluid during the filling simulation. The governing equations include the continuity equation, the momentum equation, and the energy equation. The continuity equation is written as:

$$ \frac{\partial \rho}{\partial t} + \nabla \cdot (\rho \mathbf{u}) = 0 $$

For an incompressible fluid, the continuity equation reduces to:

$$ \nabla \cdot \mathbf{u} = 0 $$

The momentum equation, also known as the Navier-Stokes equation, is expressed as:

$$ \rho \left( \frac{\partial \mathbf{u}}{\partial t} + \mathbf{u} \cdot \nabla \mathbf{u} \right) = -\nabla p + \mu \nabla^2 \mathbf{u} + \rho \mathbf{g} $$

where \(\rho\) is density, \(\mathbf{u}\) is the velocity vector, \(p\) is pressure, \(\mu\) is dynamic viscosity, and \(\mathbf{g}\) is gravitational acceleration. The energy equation accounts for heat transfer and is written as:

$$ \rho c_p \left( \frac{\partial T}{\partial t} + \mathbf{u} \cdot \nabla T \right) = \nabla \cdot (k \nabla T) + S $$

where \(c_p\) is specific heat, \(T\) is temperature, \(k\) is thermal conductivity, and \(S\) is the source term including latent heat. The volume function equation used to track the free surface is:

$$ \frac{\partial f}{\partial t} + \mathbf{u} \cdot \nabla f = 0 $$

where \(f\) is the volume fraction. When \(f = 1\), the cell is filled with melt; when \(0 < f < 1\), the cell contains a free surface; and when \(f = 0\), the cell is empty.

During solidification, heat is transferred by conduction, convection, and radiation. The Fourier law for heat conduction is:

$$ q = -k \nabla T $$

The transient heat conduction equation for the casting is:

$$ \rho c_p \frac{\partial T}{\partial t} = \nabla \cdot (k \nabla T) + \rho L \frac{\partial f_s}{\partial t} $$

where \(L\) is latent heat and \(f_s\) is the solid fraction. Convective heat transfer follows Newton’s law of cooling:

$$ q = h (T_w – T_f) $$

where \(h\) is the heat transfer coefficient, \(T_w\) is the wall temperature, and \(T_f\) is the fluid temperature. Radiative heat transfer follows the Stefan-Boltzmann law:

$$ q = \varepsilon \sigma_0 T_s^4 $$

where \(\varepsilon\) is emissivity, \(\sigma_0\) is the Stefan-Boltzmann constant, and \(T_s\) is the absolute surface temperature.

3. Formation Mechanisms of Gas Porosity and Shrinkage Porosity

Gas porosity in HPDC is usually caused by two mechanisms. The first is entrapment of air due to poor venting. When the die cavity has complex geometry, large height differences between parting surfaces, or regions where vents cannot be placed, air cannot escape. The trapped air remains in the last-filled regions and forms gas pores after solidification. The second mechanism is turbulence-induced gas entrainment. When the melt enters the cavity at excessive speed, the free surface breaks and gas is folded into the liquid. These gas pores are often irregular and can be distributed along the flow path.

Shrinkage porosity is caused by volume contraction during solidification. If the liquid metal cannot be fed through the gate or through a local reservoir, cavities form in the last-solidified regions. Uneven cooling due to wall thickness variation aggravates this problem. In the engine bracket, the remote bearing hole has a relatively thick boss and is surrounded by thinner walls. The thinner walls solidify first, while the thicker boss remains liquid for a longer time. Without sufficient feeding, shrinkage porosity forms.

The casting defects shown above are representative of the defects I observed in the engine bracket. The defects were concentrated near the remote bearing hole, where the melt arrived last and the pressure could not be effectively transmitted. X-ray inspection revealed irregular gas pores and shrinkage cavities. Sectioning confirmed that the pores were located beneath the surface and around the boss. These casting defects reduced the local load-bearing capacity and were unacceptable for the application.

4. Effect of HPDC Process Parameters on Casting Defects

I analyzed the main HPDC process parameters that influence casting defects. These parameters include intensification pressure, plunger velocity, high-speed interval, gate velocity, pouring temperature, die temperature, and cooling conditions. Among them, intensification pressure, high-speed velocity, and high-speed interval have the strongest effects on gas porosity and shrinkage porosity.

4.1 Intensification Pressure

Intensification pressure is the pressure applied to the melt during solidification. It compresses existing gas pores and promotes feeding of shrinkage cavities. The relationship between the plunger force and the intensification pressure is:

$$ F_{\text{plunger}} = P_{\text{intensification}} A_{\text{plunger}} $$

where \(F_{\text{plunger}}\) is the force exerted by the plunger, \(P_{\text{intensification}}\) is the intensification pressure, and \(A_{\text{plunger}}\) is the cross-sectional area of the plunger. A higher intensification pressure generally reduces porosity and improves density. However, excessive pressure can increase die wear and cause flash. Recommended intensification pressures for different casting types are summarized in Table 1.

Table 1. Recommended intensification pressures for HPDC.
Casting type Aluminum alloy (MPa) Zinc alloy (MPa) Brass (MPa)
Light load, low strength 30–40 13–20 30–40
Heavy load, high strength 40–80 20–30 40–60
High airtightness requirement 80–120 25–40 80–100

4.2 Plunger Velocity and Gate Velocity

The plunger velocity has two stages: slow shot and fast shot. The slow shot velocity should be low enough to avoid wave formation and gas entrainment in the shot sleeve. The fast shot velocity should be high enough to fill the cavity before the melt solidifies, but not so high that it causes severe turbulence. The relationship between the gate velocity and the plunger velocity is:

$$ v_{\text{gate}} = \frac{A_{\text{plunger}}}{A_{\text{gate}}} v_{\text{plunger}} $$

where \(v_{\text{gate}}\) is the gate velocity, \(A_{\text{plunger}}\) is the plunger cross-sectional area, \(A_{\text{gate}}\) is the gate cross-sectional area, and \(v_{\text{plunger}}\) is the plunger velocity. Recommended gate velocities for different wall thicknesses are listed in Table 2.

Table 2. Recommended gate velocities for different average wall thicknesses.
Average wall thickness (mm) Gate velocity (m/s) Average wall thickness (mm) Gate velocity (m/s)
1 46–55 5 32–40
2 42–50 6 30–37
3 38–46 7 28–34
4 34–42 8 26–32

4.3 High-Speed Interval

The high-speed interval determines the point at which the plunger switches from slow shot to fast shot. If the switch occurs too early, the melt accelerates inside the shot sleeve and may entrain gas. If the switch occurs too late, the melt loses temperature and the gate velocity becomes too low. The high-speed interval can be estimated by:

$$ H_{\text{high}} = \frac{G}{\rho A_{\text{plunger}}} + 10 $$

where \(H_{\text{high}}\) is the high-speed interval in mm, \(G\) is the total metal weight including casting and overflows, \(\rho\) is the liquid metal density, and \(A_{\text{plunger}}\) is the plunger cross-sectional area. For the engine bracket, the calculated high-speed interval was approximately 220 mm.

5. CAE Simulation of the Engine Bracket

I used a commercial casting simulation software package to simulate the filling and solidification of the engine bracket. The simulation included the casting, the gating system, the overflows, the die, the shot sleeve, and the cooling channels. I imported the 3D model, generated a mesh, assigned material properties, and defined boundary conditions. The mesh was refined near the gate and in thin-walled regions to improve accuracy. The total number of mesh elements exceeded 17 million.

5.1 Material Properties

The casting material was an AlSi9Cu3-type aluminum alloy. The die material was H13 hot-work tool steel. The thermophysical properties used in the simulation are listed in Table 3 and Table 4.

Table 3. Thermophysical properties of the aluminum alloy.
Temperature (°C) Thermal conductivity (W·m⁻¹·K⁻¹) Specific heat (J·kg⁻¹·K⁻¹) Density (kg·m⁻³)
1 140.0 820 2650
50 142.5 860 2643
100 144.5 900 2637
200 147.5 950 2619
300 152.5 980 2597
400 148.0 1050 2575
479 141.5 1150 2555
578 70.0 1000 2530
2000 70.0 1000 2095
Table 4. Thermophysical properties of H13 die steel.
Temperature (°C) Thermal conductivity (W·m⁻¹·K⁻¹) Temperature (°C) Specific heat (J·kg⁻¹·K⁻¹)
20 24.60 23 458.8
200 26.25 200 518.5
500 27.30 400 587.8
600 27.76 600 726.2
800 28.07 700 905.4
850 28.39 760 1151.1

5.2 Boundary Conditions and Initial Parameters

The heat transfer coefficients between the casting and the die, between the die and the die, and between the die and the cooling channels were defined according to the simulation database. The initial simulation parameters are listed in Table 5.

Table 5. Initial simulation parameters.
Parameter Value
Pouring temperature 650 °C
Initial die temperature 180 °C
Machine clamping force 8400 kN
Slow shot velocity 0.35 m/s
Fast shot velocity 3.5 m/s
High-speed interval 220 mm
Intensification pressure 80 MPa

5.3 Simulation Results and Defect Prediction

The filling simulation showed that the melt reached the gate at approximately 1.943 s and completed filling at approximately 1.997 s. The total filling time was about 54 ms. The melt temperature decreased from about 648 °C near the gate to about 636 °C near the remote bearing hole. The lower temperature reduced the fluidity of the melt and made it difficult to fill the remote region completely. The air pressure simulation showed that most of the cavity was well vented, but the region around the remote bearing hole had a local air pressure of approximately 3000 MPa, indicating that gas could not escape.

The solidification simulation showed that the gate solidified at about 3 s after filling. After the gate solidified, the intensification pressure could no longer be transmitted into the cavity. The remote bearing hole remained liquid for a longer time because of its larger wall thickness. Without pressure feeding, shrinkage porosity and gas porosity formed in this region. The simulation predicted that the casting defects would be concentrated around the remote bearing hole, which agreed with the actual production results.

6. Conventional Process Optimization

I used the Taguchi method to optimize the conventional HPDC process. The three factors were intensification pressure, fast shot velocity, and high-speed interval. Each factor was assigned three levels. The design variables and their ranges are listed in Table 6. The L9 orthogonal array is shown in Table 7.

Table 6. Design variables and ranges for Taguchi optimization.
Parameter Range
Intensification pressure (MPa) 80–100
Fast shot velocity (m/s) 3.0–4.0
High-speed interval (mm) 190–210
Table 7. L9 orthogonal array and experimental results.
Run Intensification pressure (MPa) Fast shot velocity (m/s) High-speed interval (mm) Maximum pore diameter (mm) Porosity (%)
A1 80 3.0 190 3.2 9.0
A2 80 3.5 200 1.9 7.2
A3 80 4.0 210 2.8 8.1
B1 90 3.0 190 3.1 8.5
B2 90 3.5 200 1.7 6.4
B3 90 4.0 210 2.0 6.9
C1 100 3.0 190 2.4 5.8
C2 100 3.5 200 1.8 4.2
C3 100 4.0 210 1.8 5.1

The results showed that increasing the intensification pressure and using a moderate fast shot velocity reduced the casting defects. The best conventional process was C2, with an intensification pressure of 100 MPa, a fast shot velocity of 3.5 m/s, and a high-speed interval of 200 mm. Under this condition, the maximum pore diameter was 1.8 mm and the porosity was 4.2%. Although the casting defects were reduced compared with the initial condition, the local porosity was still above the acceptable limit. The remote bearing hole still contained visible gas pores and shrinkage cavities. Therefore, conventional process optimization alone was insufficient to eliminate the casting defects.

7. Local Squeeze Technology

Local squeeze technology applies pressure directly to a specific region of the casting during solidification. The pressure compresses gas pores, breaks the oxide film around the pores, and forces liquid metal into the shrinkage cavities. This reduces casting defects and improves local density. I designed a local squeeze system for the engine bracket to act on the remote bearing hole.

7.1 Principle of Local Squeeze

The local squeeze process is activated after the cavity is filled. The squeeze pin moves forward and compresses the semi-solid metal around the bearing hole. The pressure is maintained for a certain duration and then released. The squeeze pressure can be estimated from the hydraulic system pressure and the area ratio:

$$ P_{\text{squeeze}} = P_{\text{system}} \left( \frac{D_{\text{cylinder}}}{D_{\text{pin}}} \right)^2 $$

where \(P_{\text{squeeze}}\) is the squeeze pressure at the pin tip, \(P_{\text{system}}\) is the hydraulic system pressure, \(D_{\text{cylinder}}\) is the cylinder bore diameter, and \(D_{\text{pin}}\) is the squeeze pin diameter. For a system pressure of 16 MPa, a cylinder bore of 50 mm, and a pin diameter of 10.5 mm, the calculated squeeze pressure is approximately 360 MPa. The force acting on the pin is:

$$ F_{\text{pin}} = P_{\text{squeeze}} \frac{\pi D_{\text{pin}}^2}{4} $$

which gives a force of approximately 3000 kN.

7.2 Design of Squeeze Pin, Sleeve, and Cylinder

I designed the squeeze pin and sleeve to withstand high temperature and high pressure. The squeeze pin was made of SKD61 hot-work tool steel, heat treated to HRC 40–45, and then coated with a D+ coating to increase surface hardness. The final hardness was measured at HRC 50–55. The pin diameter was 10.5 mm to match the bearing hole. The clearance between the pin and the sleeve was kept between 0.02 and 0.04 mm to prevent molten metal from entering the gap and to allow smooth sliding. The sleeve was fixed to the die insert by a locking plate. The squeeze cylinder had a bore of 50 mm and a maximum stroke of 20 mm. The cylinder was connected to the pin through upper and lower clamping rings.

Table 8. Key dimensions of the local squeeze system.
Component Dimension or parameter Value
Squeeze pin Diameter 10.5 mm
Squeeze pin Material SKD61, D+ coated
Squeeze pin Hardness HRC 50–55
Squeeze sleeve Clearance with pin 0.02–0.04 mm
Squeeze cylinder Bore diameter 50 mm
Squeeze cylinder Maximum stroke 20 mm
System pressure Hydraulic pressure 16 MPa
Squeeze pressure At pin tip 360 MPa

7.3 Local Squeeze Process Sequence

The local squeeze-assisted HPDC cycle is as follows. First, the die is closed and the shot sleeve is filled with a measured amount of molten aluminum. Second, the plunger advances slowly and then rapidly to fill the cavity. During filling, the squeeze pin is retracted so that its front face is 1–2 mm away from the cavity surface. Third, after the cavity is filled, the intensification pressure is applied. Fourth, after a preset delay time, the squeeze cylinder pushes the pin forward. The pin compresses the semi-solid metal around the bearing hole and forms the hole. Fifth, the squeeze pressure is held for a preset duration. Finally, the squeeze pin is retracted, the die opens, and the casting is ejected.

7.4 Determination of Squeeze Timing

The squeeze delay time is the interval between the end of filling and the start of squeezing. The squeeze duration is the time during which the squeeze pressure is maintained. These parameters must be chosen so that the metal around the bearing hole is in a semi-solid state. If the delay is too short, the metal is still liquid and the squeeze pin may not build up enough pressure. If the delay is too long, the metal becomes solid and the pin cannot move forward. I used the solid fraction curve of the aluminum alloy to estimate the appropriate temperature range. The solid fraction as a function of temperature is shown in Table 9.

Table 9. Solid fraction of the aluminum alloy near the solidification range.
Temperature (°C) Solid fraction (%)
580 0
570 19
560 37
550 52
540 65
530 78
520 88
510 95
500 99
480 100

Based on the temperature simulation, the metal near the bearing hole cooled from about 580 °C to about 560 °C within 1 s after filling. Therefore, a delay time of about 1 s placed the metal in the semi-solid range with a solid fraction between 19% and 37%. This was considered suitable for local squeezing.

8. Experimental Results and Discussion

I conducted local squeeze-assisted HPDC experiments on a cold-chamber die casting machine. The casting pressure was kept at 100 MPa, and the squeeze pressure was 360 MPa. I varied the squeeze delay time and the squeeze duration. I measured the squeeze depth, the maximum pore diameter, and the local porosity. The results are summarized in Table 10 and Table 11.

Table 10. Effect of squeeze delay time on squeeze depth.
Delay time (s) Squeeze depth, trial 1 (mm) Squeeze depth, trial 2 (mm) Squeeze depth, trial 3 (mm) Average squeeze depth (mm)
0.10 8.05 7.90 8.03 7.99
0.30 6.91 7.02 7.35 7.09
0.50 5.71 6.60 5.80 6.04
0.75 5.20 5.34 5.22 5.25
1.00 5.05 4.95 3.96 4.80
1.20 2.50 1.86 2.41 2.27
1.50 1.21 0.68 1.10 0.99
2.00 0.78 0.21 0.68 0.56
Table 11. Effect of squeeze duration on casting defects.
Delay time (s) Squeeze duration (s) Average squeeze depth (mm) Maximum pore diameter (mm) Porosity (%)
1.0 0.5 4.80 2.35 4.3
1.0 1.0 4.86 2.29 3.9
1.0 1.5 5.01 1.97 2.9
1.0 3.0 5.59 1.41 1.2
1.0 4.0 5.80 0.72 1.0
1.0 5.0 6.45 0.46 0.6

The results show that the squeeze depth decreased as the delay time increased. When the delay time was 0.1 s, the metal was almost fully liquid, and the squeeze pin could move forward easily, resulting in a large squeeze depth of 7.99 mm. However, because the metal was too fluid, the pressure did not effectively compress the gas pores. When the delay time was 2.0 s, the solid fraction was high, and the squeeze depth was only 0.56 mm. The pin could not move enough to compress the casting defects. The optimal delay time was between 0.85 and 1.0 s. At 1.0 s, the metal was in the semi-solid state, and the squeeze pin could still move forward while applying enough pressure to reduce casting defects.

The squeeze duration also had a strong effect on casting defects. A longer squeeze duration allowed the pressure to act on the semi-solid metal for a longer time, which promoted pore compression and feeding. When the squeeze duration was 0.5 s, the maximum pore diameter was 2.35 mm and the porosity was 4.3%, which did not meet the acceptance level. When the squeeze duration was increased to 5.0 s, the maximum pore diameter decreased to 0.46 mm and the porosity decreased to 0.6%. This met the level 1 acceptance criterion for the relevant wall thickness range. A squeeze duration longer than 5 s was not beneficial because the casting began to solidify completely and the pin could become stuck. In one trial with a squeeze duration of 7 s, the remote ear of the bracket was torn when the die opened.

The final optimal parameters were: casting pressure 100 MPa, squeeze pressure 360 MPa, squeeze delay time 1.0 s, and squeeze duration 5.0 s. Under these conditions, the casting surface was smooth, the internal casting defects were significantly reduced, and the local porosity was 0.6%. The maximum pore diameter was 0.46 mm. These results demonstrated that local squeeze-assisted HPDC can effectively reduce casting defects that cannot be eliminated by conventional process optimization alone.

9. Summary of Findings

I found that the main causes of casting defects in the engine bracket were the complex die cavity, the large height difference between parting surfaces, the inability to place vents near the remote bearing hole, and the early solidification of the gate. These factors prevented gas from escaping and prevented intensification pressure from reaching the last-filled region. The casting defects were concentrated around the remote bearing hole.

I also found that conventional process optimization using the Taguchi method could reduce casting defects but could not eliminate them. The best conventional process reduced the maximum pore diameter to 1.8 mm and the porosity to 4.2%, which was still above the acceptable limit. Therefore, local squeeze technology was necessary.

The local squeeze system was designed with a 10.5 mm squeeze pin, a 50 mm cylinder bore, and a 20 mm stroke. The squeeze pressure was 360 MPa. The optimal squeeze delay time was 1.0 s, and the optimal squeeze duration was 5.0 s. Under these conditions, the maximum pore diameter was reduced to 0.46 mm and the porosity was reduced to 0.6%. The casting defects met the level 1 acceptance criterion.

Table 12. Comparison of casting defects before and after local squeeze.
Condition Maximum pore diameter (mm) Porosity (%) Acceptance
Initial HPDC 3.2 9.0 Not acceptable
Optimized HPDC 1.8 4.2 Not acceptable
Local squeeze-assisted HPDC 0.46 0.6 Acceptable

10. Conclusions

I developed a complete workflow for reducing casting defects in an HPDC engine bracket. The workflow combined theoretical analysis, CAE simulation, Taguchi process optimization, local squeeze system design, and experimental validation. The main conclusions are as follows.

First, the casting defects in the engine bracket were caused by poor venting and insufficient pressure transmission near the remote bearing hole. The simulation predicted the defect locations accurately, and the experimental results confirmed the prediction. The gas pressure in the last-filled region was much higher than atmospheric pressure, and the gate solidified before the remote region finished solidifying.

Second, conventional process optimization reduced the casting defects but did not reduce them to an acceptable level. The best conventional parameters were an intensification pressure of 100 MPa, a fast shot velocity of 3.5 m/s, and a high-speed interval of 200 mm. Under these conditions, the porosity was still 4.2%.

Third, local squeeze-assisted HPDC effectively reduced the casting defects. The squeeze pin and sleeve were designed with a clearance of 0.02–0.04 mm. The squeeze pressure was 360 MPa. The optimal delay time was 1.0 s, and the optimal duration was 5.0 s. The maximum pore diameter was reduced to 0.46 mm, and the porosity was reduced to 0.6%.

Fourth, the local squeeze process must be carefully timed. If the delay time is too short, the metal is too fluid and the pressure does not compress the pores effectively. If the delay time is too long, the metal is too solid and the pin cannot move. A delay time of about 1.0 s placed the metal in the semi-solid range and produced the best results.

Finally, I established an efficient production method that combines local squeeze technology with CAE analysis and HPDC. This method can reduce casting defects, improve product quality, and increase production efficiency. The results provide a practical reference for reducing casting defects in similar lightweight aluminum components.