In my daily work with precision casting, I have repeatedly seen how shrinkage cavities and shrinkage porosity can destroy the performance of an otherwise well-made investment casting. Precision casting is a near-net-shape process, and because of that, every internal discontinuity is magnified in importance. When a precision casting is intended for wear resistance, pressure tightness, fatigue resistance, or high contact loading, a shrinkage defect may become the starting point for early failure. I have therefore treated shrinkage control as one of the central tasks of precision casting process design, not as a secondary correction after pouring.
In precision casting, molten metal is poured into a hot ceramic shell. The metal then loses heat through the shell, through the gating system, and through radiation from exposed surfaces. As the metal cools from the pouring temperature to room temperature, it passes through liquid contraction, solidification contraction, and solid contraction. The first two contraction stages are the ones that create a demand for feed metal. If that demand is not satisfied, a concentrated cavity or a dispersed network of porosity remains in the last region to solidify. In precision casting, that region is often a hot spot, a thick section, an isolated boss, or a corner where the shell removes heat slowly.

Classification and appearance of shrinkage defects
From my inspection experience, shrinkage defects in precision casting can be grouped into concentrated shrinkage cavities and dispersed shrinkage porosity. A concentrated shrinkage cavity is a relatively large, irregular void. Its internal surface is rough, and under magnification it may show developed dendritic arms. When the cavity reaches the external surface, I call it an external shrinkage cavity. When it remains inside the casting, I call it an internal shrinkage cavity. When it forms in a re-entrant corner, I call it a corner shrinkage cavity. These three forms have essentially the same origin; they differ mainly in location and in how they are exposed during finishing.
| Defect form | Typical location | Visual character | Main cause in precision casting |
|---|---|---|---|
| External shrinkage cavity | Open surface, riser contact, top face | Rough irregular depression or hole | Last solidifying metal exposed to air without feed |
| Internal shrinkage cavity | Hot spot, thick section, isolated mass | Internal void with dendritic surface | Insufficient directional solidification and feeding |
| Corner shrinkage cavity | Re-entrant corner, junction of walls | Localized cavity at a slow-cooling corner | Poor local heat extraction and late solidification |
| Shrinkage porosity | Dendritic interstices, dispersed hot spots | Fine scattered pores, often interdendritic | Gas evolution and limited liquid feeding |
Contraction stages and their mathematical description
I always begin a shrinkage analysis by separating the total volumetric contraction into three stages. In precision casting, this separation is important because liquid contraction and solidification contraction create the cavity, while solid contraction changes the final dimensions and may open cracks. For a steel precision casting, the liquid volumetric contraction can be written as
$$ \varepsilon_{V,\ell} = \alpha_{V,\ell}(t_p – t_L) \times 100\% $$
where \(\varepsilon_{V,\ell}\) is the liquid volumetric contraction, \(\alpha_{V,\ell}\) is the average volumetric contraction coefficient of the liquid, \(t_p\) is the pouring temperature, and \(t_L\) is the liquidus temperature. For carbon steel, I commonly use \(\alpha_{V,\ell} = 1.6 \times 10^{-4}\,\mathrm{^\circ C^{-1}}\). The term \(t_p – t_L\) is the superheat. It is one of the most powerful variables in precision casting because it controls both fluidity and the amount of liquid contraction.
The solidification contraction occurs between the liquidus and solidus. Its value depends strongly on composition. In my tables for carbon steel, I use values such as those shown below.
| Carbon content, \(\omega_C\) (%) | 0.10 | 0.35 | 0.45 | 0.70 |
|---|---|---|---|---|
| Solidification contraction, \(\varepsilon_{V,c}\) (%) | 2.0 | 3.0 | 4.3 | 5.3 |
The solid contraction occurs from the solidus to room temperature. I express it as
$$ \varepsilon_{V,s} = \alpha_{V,s}(t_S – t_R) \times 100\% $$
and the corresponding linear contraction is
$$ \varepsilon_{\ell} = \alpha_{\ell}(t_S – t_R) \times 100\% $$
where \(t_S\) is the solidus temperature, \(t_R\) is room temperature, \(\varepsilon_{V,s}\) is the solid volumetric contraction, and \(\varepsilon_{\ell}\) is the linear solid contraction. For steel, the linear solid contraction is approximately one third of the volumetric solid contraction, and a common value is about \(2.4\%\). The solid linear contraction also depends on carbon and other elements.
| Carbon content, \(\omega_C\) (%) | Pre-pearlite contraction, \(\varepsilon_{\text{pre}}\) (%) | Eutectoid expansion, \(\varepsilon_{\gamma \rightarrow \alpha}\) (%) | Post-pearlite contraction, \(\varepsilon_{\text{post}}\) (%) | Total solid linear contraction, \(\varepsilon_{\ell}\) (%) |
|---|---|---|---|---|
| 0.08 | 1.42 | 0.11 | 1.16 | 2.47 |
| 0.14 | 1.51 | 0.11 | 1.06 | 2.46 |
| 0.35 | 1.47 | 0.11 | 1.04 | 2.40 |
| 0.45 | 1.39 | 0.11 | 1.07 | 2.35 |
| 0.55 | 1.35 | 0.09 | 1.05 | 2.31 |
| 0.90 | 1.21 | 0.01 | 0.98 | 2.18 |
The total volumetric contraction from pouring to room temperature is therefore
$$ \varepsilon_{V,\mathrm{total}} = \varepsilon_{V,\ell} + \varepsilon_{V,c} + \varepsilon_{V,s} $$
For a medium-carbon steel precision casting, I have used the following example. With a superheat of about \(100\,\mathrm{^\circ C}\), the liquid contraction may be \(1.6\%\), the solidification contraction may be \(3.0\%\), and the solid contraction may be \(7.2\%\). The total is then
$$ \varepsilon_{V,\mathrm{total}} = 1.6\% + 3.0\% + 7.2\% = 11.8\% $$
In real precision casting, this total is not always fully expressed as an internal void. Gas evolution can form porosity, the shell and core can restrain contraction, and the casting geometry can impose non-uniform cooling. All of these factors reduce or redistribute the apparent contraction. Nevertheless, the calculation gives me a first estimate of the feed metal demand and explains why a precision casting with a high superheat and a poorly fed hot spot is so vulnerable.
Mechanism of concentrated shrinkage formation
The formation of a concentrated shrinkage cavity in precision casting can be described with a cylindrical section. When the metal enters the mold cavity, most heat is removed through the shell. A temperature gradient develops from the shell surface toward the thermal center. The outermost liquid cools below the liquidus first and freezes as a thin skin. As the skin grows inward, the remaining liquid contracts. Because the solid skin is already relatively strong, the liquid level falls and a gap forms at the top. The gap is not repaired unless feed metal can flow into it. With continued cooling, the solid shell thickens, the liquid volume decreases further, and the void becomes larger. At the end of solidification, a conical or irregular cavity remains in the last region to freeze. During final cooling, the solid casting contracts and both the external dimensions and the cavity volume decrease slightly.
The same mechanism applies in precision casting when the casting has a hot spot that is isolated from the gating system. The hot spot remains liquid after the surrounding thin walls have solidified. If the gating system freezes before the hot spot, no feed metal can reach it. A cavity then forms. If the hot spot is connected to a riser that remains liquid, the cavity can be transferred into the riser. This is the basis of directional solidification in precision casting.
| Stage | What happens in precision casting | Effect on shrinkage |
|---|---|---|
| Initial fill | Molten metal fills the shell cavity and gating system | Liquid contraction begins immediately |
| Skin formation | Outer layer cools below liquidus and freezes | Liquid level drops because of contraction |
| Shell growth | Solidification front moves inward | Liquid volume decreases, void grows |
| Hot spot isolation | Thin sections freeze before thick sections | Feed path may close prematurely |
| Final solidification | Last liquid freezes without feed | Concentrated cavity or porosity remains |
Locations where shrinkage defects appear in precision casting
In my experience, shrinkage defects in precision casting are not randomly distributed. They appear in regions that solidify last and cannot be fed. These regions include thermal hot spots, thick walls, isolated bosses, junctions of walls, re-entrant corners, and areas close to a slow-cooling shell. The position of the ingate also matters because it controls the local temperature field. If the ingate is placed on a thin wall, it may not feed the thick section. If it is placed on a thick section, it may create a new hot spot at the junction. The arrangement of patterns on the tree also changes heat flow. A pattern in the center of a cluster may cool more slowly than a pattern on the outside. This is why I always consider the whole precision casting tree, not only the individual part.
Several methods can be used to predict shrinkage locations in precision casting. I use isotherm plotting, the inscribed circle method, sectioning, and computer simulation. The inscribed circle method is simple and effective for estimating hot spots. I draw the largest possible circle in each section. The section with the largest circle tends to solidify last. If the feeding path is short, a cavity may form there. Computer simulation is more powerful because it shows the filling and solidification sequence. I use it to observe the last liquid regions and to test gating changes before cutting metal.
| Prediction method | Principle | Advantage in precision casting | Limitation |
|---|---|---|---|
| Isotherm plotting | Map temperature contours during solidification | Shows thermal gradients and hot spots | Requires thermal data and experience |
| Inscribed circle | Compare largest circles in sections | Fast, simple, useful for hot spot ranking | Does not include gating effects |
| Sectioning | Cut and inspect actual castings | Confirms defect location and size | Destructive and time-consuming |
| Computer simulation | Solve filling and solidification numerically | Predicts shrinkage and porosity before trial | Needs accurate properties and boundary conditions |
Causes of shrinkage defects in precision casting
I have found that shrinkage defects in precision casting usually arise from a combination of design, material, and process factors. The most common cause is an incorrectly designed gating system. If the gating system does not promote directional solidification, the last liquid cannot be fed. If the ingate is too small, it freezes early. If the runner is too small, it cannot supply enough feed metal. If the riser is too small, its own shrinkage cannot be transferred away from the casting. In precision casting, the gating system often serves as the riser, so its dimensions directly control feeding.
Another major cause is an unreasonable casting structure. Abrupt changes in section size cause thin sections to freeze before thick sections. An isolated thick section has no feed path. A fillet that is too small creates a sharp transition and a hot spot. A fillet that is too large creates a new hot spot. Parts that were originally designed for forging or welding may not have been redesigned for precision casting. In such cases, the geometry may contain thick masses and isolated hot spots that are difficult to feed.
The shrinkage of the alloy itself also matters. A larger liquid contraction and a larger solidification contraction produce a larger cavity if feed is insufficient. However, the relationship is not always simple. If the gating system has good feeding ability, a higher superheat may improve feeding and reduce the final cavity, even though the liquid contraction increases. If the superheat is too low, the gating system may freeze early and lose its feeding ability. Therefore, I do not simply lower the pouring temperature to reduce contraction. I balance superheat against feeding distance and shell temperature.
Pouring conditions are another factor. A faster pouring speed shortens the heat loss time. The liquid temperature at the end of pouring is higher, so the liquid contraction increases. At the same time, the earlier metal has less time to be fed by later metal. The final cavity volume therefore tends to increase. The cooling capacity of the shell also matters. A shell with poor cooling capacity slows solidification and reduces the amount of feed metal that can be supplied before the feed path closes. Local heat dissipation is especially important at corners. A re-entrant corner loses heat slowly, so it remains liquid longer. If it is not fed, a corner shrinkage cavity forms. Finally, an insufficient pressure head reduces the flow of feed metal and worsens feeding.
| Cause | Mechanism in precision casting | Typical result |
|---|---|---|
| Poor gating design | Feed path freezes early or riser is inadequate | Internal or external shrinkage cavity |
| Abrupt section change | Thin wall freezes before thick section | Hot spot isolation and internal cavity |
| Isolated thick section | No liquid feed path from riser | Large concentrated cavity |
| Improper fillet radius | Small radius creates hot spot; large radius creates new hot spot | Shrinkage at junction |
| High liquid contraction | Superheat increases demand for feed metal | Larger cavity if feeding is poor |
| High solidification contraction | Volume deficit between liquidus and solidus | Interdendritic porosity |
| Fast pouring | Less heat loss, higher final liquid temperature | Larger concentrated cavity |
| Poor shell cooling | Slow solidification, late feed path closure | Increased shrinkage volume |
| Poor local cooling | Corner remains liquid longer | Corner shrinkage cavity |
| Low pressure head | Reduced feed metal flow | Incomplete feeding |
Prevention by directional solidification
The basic rule I follow in precision casting is to make the casting solidify directionally toward the gating system or riser. The shrinkage cavity should be moved out of the casting and into the gating system, where it can be removed by cutting. Directional solidification requires a temperature gradient that decreases from the riser toward the far end of the casting. The last liquid should be in the riser, not in the casting. To achieve this, I control the gating system, the casting geometry, the shell temperature, the pouring temperature, and the local cooling conditions.
Correct gating system design
In precision casting, the gating system usually includes a pouring cup, a sprue, a runner, and an ingate. Sometimes a slag trap, a buffer, or a vent is added. The pouring cup receives the metal and establishes a pressure head. The sprue supports the shell and often acts as a riser. The runner distributes metal and can also feed. The ingate connects the gating system to the casting and controls both filling and feeding. Because the ingate is the final connection, it is the most critical element in shrinkage control.
| Gating component | Function in precision casting | Recommended area relationship |
|---|---|---|
| Pouring cup | Receive metal, establish pressure head | Top surface distance to pattern: 70 to 100 mm |
| Sprue | Support shell, act as riser | Area = 1.4 times total ingate area |
| Runner | Distribute metal, trap slag, feed | 1.1 to 1.3 times sprue area if feeding; 0.7 to 1.0 if not feeding |
| Ingate | Connect gating to casting, control filling and feeding | Determined by hot spot size: \(D_{\text{ingate}} = K D_{\text{hot spot}}\), \(K = 0.7\) to \(0.9\) |
When I design an ingate for precision casting, I consider position, number, shape, length, and cross-sectional size. The position must avoid direct impact on cores and thin shell sections. It must also be placed so that the hot spot is fed. From the feeding point of view, the best position is often at the hot spot or adjacent to it. However, if the ingate is placed directly on a thick section, the junction itself may become a hot spot. I therefore use a gradual transition and, when necessary, a pad or fillet.
The number of ingates depends on the complexity of the precision casting. A single ingate is usually preferred because it simplifies pattern making, shell building, dewaxing, pouring, and cleaning. However, if the casting has several isolated hot spots or if it is large and complex, I use two or more ingates. The shape can be rectangular, circular, square, or fan-shaped. The length must be sufficient for easy removal. For a knock-off ingate, I use about 8 to 12 mm. For a gas-cut ingate, I use about 10 to 15 mm. The cross-section can be estimated by the hot spot circle method or by the equivalent hot spot method. In the hot spot circle method,
$$ D_{\text{ingate}} = K D_{\text{hot spot}} $$
with \(K\) usually between 0.7 and 0.9. If the ingate is too large, the ingate neck remains liquid until the end and may itself produce a cavity at the casting connection. If it is too small, it freezes early and cannot feed the hot spot.
| Ingate parameter | Recommendation for precision casting | Reason |
|---|---|---|
| Position | At or near hot spot, avoid core impact | Promotes feeding and smooth filling |
| Number | Usually one; more for multiple hot spots | Balances simplicity and feeding |
| Shape | Rectangular, circular, square, fan | Matches local geometry and flow needs |
| Length | 8 to 12 mm for knock-off; 10 to 15 mm for gas cut | Allows removal without damaging casting |
| Cross-section | \(D_{\text{ingate}} = K D_{\text{hot spot}}\), \(K = 0.7\) to \(0.9\) | Controls feeding and freezing time |
Improving casting structure for precision casting
I always review the casting structure before finalizing the precision casting process. The first step is to identify all hot spots and divide the casting into feeding regions. Then I adjust wall thickness, fillets, and allowances. If a section is too thick, I reduce it when the design allows. If a section is too thin, I increase it to avoid premature freezing. The goal is to make the wall thickness as uniform as possible and to provide a clear feed path. Fillets should be large enough to avoid sharp transitions but not so large that they create new hot spots.
When normal changes are not enough, I use padding. Padding is a local increase in thickness near the riser. It creates a positive temperature gradient toward the riser and increases the feeding channel. For a top-poured precision casting, the padding width increases with height when the wall thickness is fixed. When the height is fixed, a thinner wall requires a wider feeding channel. Padding increases machining allowance, so I use it only when necessary. Excessive padding can reduce the economic advantage of precision casting.
| Structural measure | Action | Expected effect in precision casting |
|---|---|---|
| Uniform wall thickness | Reduce thick sections and increase thin sections | More even cooling, fewer isolated hot spots |
| Proper fillet radius | Avoid too small or too large radii | Prevents hot spot at junction |
| Feeding region analysis | Divide casting according to hot spots | Places ingates and risers correctly |
| Padding | Add thickness near riser | Improves feeding channel and gradient |
| Redesign for casting | Replace forging or welded geometry with casting-friendly shape | Reduces isolated masses and shrinkage risk |
Reducing alloy contraction
I try to select an alloy with a favorable solidification range and low contraction when the service conditions permit. Once the alloy is fixed, I control the process variables that affect contraction. The most important are pouring temperature, shell temperature, and cooling rate. A high pouring temperature increases liquid contraction. If feeding is adequate, it may still improve the final result by keeping the gating system liquid. A low pouring temperature reduces liquid contraction but may freeze the gating system too early. Therefore, I use the lowest pouring temperature that still provides reliable filling and feeding. I also control shell temperature. A hot shell improves filling but slows cooling and may increase shrinkage. A cold shell increases the temperature gradient and can improve directional solidification, but it may also cause cold shuts or incomplete filling.
In practice, I use the following relationship as a guide:
$$ \text{Feeding ability} \propto \frac{A_{\text{feed}} \rho g h}{L_f} $$
where \(A_{\text{feed}}\) is the effective feed channel area, \(\rho\) is density, \(g\) is gravitational acceleration, \(h\) is pressure head, and \(L_f\) is the flow resistance in the feed path. This expression reminds me that feeding is not only a matter of volume. It also depends on the pressure head and the resistance of the channel. In precision casting, the feed channel is often narrow and winding, so flow resistance can be significant.
| Process variable | Effect on contraction | Effect on feeding | Practical direction |
|---|---|---|---|
| Higher pouring temperature | Increases liquid contraction | Keeps gating liquid longer | Use only as needed for filling and feeding |
| Lower pouring temperature | Reduces liquid contraction | May freeze gating early | Avoid excessive superheat, but do not underheat |
| Higher shell temperature | Slower cooling, more time for feed | May reduce thermal gradient | Balance filling and directional solidification |
| Lower shell temperature | Faster cooling, stronger gradient | May freeze feed path early | Use with adequate gating and pouring control |
Deoxidation and gas control
In precision casting, gas evolution during solidification can either increase or decrease shrinkage porosity. If gas forms bubbles that cannot escape, the bubbles may occupy space that would otherwise become a shrinkage cavity, reducing the apparent cavity volume but increasing dispersed porosity. This is not a desirable trade-off. I therefore insist on sufficient deoxidation during melting. Clean metal has fewer gas nuclei, better fluidity, and more predictable feeding. In steel precision casting, I use standard deoxidation practice and verify the results through sectioning and mechanical testing.
Pouring conditions and feeding
Pouring conditions have a direct effect on shrinkage in precision casting. When the pouring speed is too high, the metal enters the mold quickly, the shell has less time to remove heat, and the liquid temperature at the end of pouring is higher. The liquid contraction increases, and the earlier metal receives less feed from the later metal. The result is a larger concentrated shrinkage cavity. When the pouring speed is too low, the metal may freeze before the mold is filled, or the gating system may freeze before feeding is complete. I therefore use controlled pouring. For large clusters, I often use a fast-first, slow-later, and final top-up sequence. For top gating, I use a higher pouring temperature and a slower pouring speed. For bottom gating, I use a lower pouring temperature and a faster pouring speed.
| Pouring condition | Effect in precision casting | Recommended practice |
|---|---|---|
| High pouring speed | Less heat loss, higher final liquid temperature, larger cavity | Avoid unless filling requires it |
| Low pouring speed | More heat loss, risk of cold shut and early freeze | Use controlled slow pour with sufficient superheat |
| Top gating | Good directional gradient from top to bottom | Higher pouring temperature, slower speed |
| Bottom gating | Smooth filling, but reversed thermal gradient | Lower pouring temperature, faster speed |
| Large cluster | Long pouring time and complex heat flow | Fast first, slow later, final top-up |
Local cooling and shell design
Local cooling is one of the most practical ways to reduce shrinkage in precision casting. A re-entrant corner often cools more slowly than the surrounding walls because the shell mass is greater and radiation is partly blocked. If the corner remains liquid after the feed path closes, a corner shrinkage cavity forms. I improve local cooling by placing the pattern near the edge of the tree, by keeping a suitable distance between patterns, and by using chills when necessary. For precision casting, I prefer chills made of brass or stainless steel because carbon steel may oxidize during shell firing and bond poorly. A chill placed near the corner increases the local heat extraction rate and helps the corner solidify earlier or at the same time as the adjacent wall.
| Local cooling method | How it works | Best use in precision casting |
|---|---|---|
| Pattern spacing | Reduces mutual heating between patterns | Clusters with multiple parts |
| Edge placement | Exposes hot spot to better radiation and cooling | Single heavy part on a tree |
| Chill insertion | Increases local heat extraction | Re-entrant corners and isolated hot spots |
| Shell thickness control | Changes local thermal resistance | Areas with slow cooling |
Pressure head and riser design
An adequate pressure head improves feeding in precision casting. The higher the pressure head, the faster the feed metal can flow and the more effective the feeding. However, increasing riser diameter and height alone does not always solve the problem. If the riser is too high, it may only feed the lower part of its own volume, and a secondary shrinkage cavity may remain. The effective feeding distance also decreases as wall thickness increases. In precision casting, I often combine an insulating riser with a covering flux or exothermic agent. The covering agent reduces heat loss from the top of the riser and delays skin formation, which helps prevent a secondary cavity. When ordinary gravity feeding is not enough, I consider centrifugal casting or pressure-assisted pouring.
The effective feeding distance can be estimated from the wall thickness. As a general trend,
$$ L_{\text{eff}} \propto \frac{1}{e} $$
where \(L_{\text{eff}}\) is the effective feeding distance and \(e\) is the wall thickness. This means that a thicker wall requires a shorter relative feeding distance. In precision casting, this relationship explains why heavy sections are so difficult to feed with a single small riser. I may need a larger riser, a chilled section, or a revised geometry.
| Pressure head measure | Effect | Caution |
|---|---|---|
| Increase sprue height | Raises pressure and improves feeding flow | May increase mold height and metal consumption |
| Increase riser diameter | Provides more feed metal | May create a new hot spot if too large |
| Insulating riser | Keeps riser liquid longer | Needs proper shell and insulation design |
| Exothermic covering | Reduces top heat loss and secondary shrinkage | Must be compatible with alloy and shell |
| Centrifugal or pressure pouring | Improves feeding when gravity is insufficient | Adds process complexity |
Interaction with residual stress and cracking
I must also remember that directional solidification creates temperature differences. A strong gradient helps feeding, but it also produces thermal stress. If the casting is restrained by the shell or by its own geometry, the stress may cause distortion or cracking. In precision casting, thin walls and complex cores are especially sensitive. Therefore, I do not pursue directional solidification blindly. I balance feeding against stress. Sometimes a small amount of dispersed porosity is less harmful than a crack. The optimum process is the one that meets the service requirements at acceptable cost and yield.
Application case: rare-earth modification in a wear-resistant precision casting
I once worked on a critical precision casting weighing about 16 kg. The part was used in a mining device, and its service life was expected to exceed a certain large advance distance. In actual service, however, it failed after only a fraction of that distance. The failure was caused by severe shrinkage cavities and axial porosity on the wear surface. The porosity reduced the local hardness and toughness, and the wear rate increased. I therefore focused on reducing shrinkage in the precision casting and improving the alloy.
I selected a low-alloy steel with rare-earth addition. The rare earth improves fluidity, increases feeding ability, reduces shrinkage cavities and porosity, and improves mechanical properties. It also has purification, modification, and alloying effects. The material was designated ZG20CrMnMoRe, and its chemical composition is shown below.
| Material | C | Si | Mn | Cr | Mo | P | S | Re addition |
|---|---|---|---|---|---|---|---|---|
| ZG20CrMnMoRe | 0.15 to 0.25 | 0.40 to 0.75 | 0.90 to 1.20 | 1.10 to 1.40 | 0.20 to 0.30 | ≤0.04 | ≤0.04 | 0.15 |
I tested three rare-earth addition methods. The results showed that the ladle injection method gave the best recovery and the most stable residual content. The furnace insertion method and the furnace addition method gave lower and less consistent recovery. The ladle injection method also produced more stable mechanical properties.
| Addition method | Rare-earth recovery (%) | Rare-earth residual (%) |
|---|---|---|
| Furnace insertion | Decreased with pouring time | Decreased with pouring time |
| Furnace addition | 15 to 25 | 0.02 to 0.04 |
| Ladle injection | 50 to 80 | 0.08 to 0.12 |
I then investigated the effect of rare-earth addition on mechanical properties. The same base metal was used, and different amounts of rare-earth alloy were added by ladle injection: 0, 0.15%, 0.30%, and 0.40%. The test bars were normalized, tempered, carburized, quenched, and tempered. The results showed that 0.15% addition gave the best combination of properties and cost. At this level, the recovery was 50% to 80%, and the residual rare-earth content was 0.08% to 0.12%.
| Rare-earth addition (%) | 0 | 0.15 | 0.30 | 0.40 |
|---|---|---|---|---|
| Tensile strength, sample 1 (MPa) | 217 | 236 | 243 | 234 |
| Tensile strength, sample 2 (MPa) | 212 | 312 | 319 | 288 |
| Impact toughness, sample 1 (J/cm²) | 1.08 | 1.58 | 1.63 | 1.50 |
| Impact toughness, sample 2 (J/cm²) | 3.07 | 5.17 | 5.73 | 3.8 |
I poured a set of production castings with and without rare-earth addition. The rare-earth-modified precision castings showed no gas porosity rejects in the test group, while the unmodified group had gas porosity rejects. After nitric acid etching, the unmodified castings showed severe shrinkage cavities and porosity, while the modified castings showed only slight porosity. This confirmed that rare earth improved feeding and reduced gas-related defects in the precision casting.
| Casting type | Number poured | Gas porosity rejects | Structural density after etching |
|---|---|---|---|
| Without rare earth | 10 | 2 | Severe shrinkage cavities and porosity |
| With rare earth | 15 | 0 | Slight porosity visible |
The chemical composition of the modified and unmodified steels was checked. The rare-earth residual in the modified steel was about 0.102%, while the unmodified steel had none. The modified steel also had lower sulfur, which is consistent with the purifying effect of rare earth.
| Material | C | Si | Mn | Cr | Mo | S before Re | S after Re | Re residual |
|---|---|---|---|---|---|---|---|---|
| ZG20CrMnMo | 0.24 | 0.35 | 1.00 | 1.32 | 0.23 | 0.029 | — | 0 |
| ZG20CrMnMoRe | 0.24 | 0.57 | 1.00 | 1.32 | 0.23 | 0.029 | 0.015 | 0.102 |
Mechanical testing after heat treatment showed that the rare-earth-modified steel had higher bending strength and much higher impact toughness. The true carburized case, which represents the carburized layer, improved by about 50%. The false carburized case, which represents the core, improved by nearly three times.
| Material | Bending strength, true carburized | Bending strength, false carburized | Impact toughness, true carburized | Impact toughness, false carburized |
|---|---|---|---|---|
| ZG20CrMnMo | 187 | 218 | 1.2 | 2.2 |
| ZG20CrMnMoRe | 198 | 288 | 1.8 | 6.4 |
Wear tests were also performed. The rare-earth-modified steel had slightly higher hardness and lower mass loss at all test intervals. At 40,000 revolutions, the mass loss was about 3.2678 g for the modified steel and about 3.7872 g for the unmodified steel. The dimensional reduction was also smaller. This confirmed that the reduction in shrinkage and porosity improved wear resistance.
| Material | Hardness (HRC) | 5,000 revolutions, mass loss (g) | 20,000 revolutions, mass loss (g) | 40,000 revolutions, mass loss (g) | 40,000 revolutions, dimensional reduction (mm) |
|---|---|---|---|---|---|
| ZG20CrMnMo | 59 to 61 | 0.2087 | 1.7770 | 3.7872 | 0.8810 |
| ZG20CrMnMoRe | 60 to 62 | 0.1557 | 1.2368 | 3.2678 | 0.7170 |
The field trial confirmed the laboratory results. Two modified precision castings were installed in a mining machine under hard rock conditions. Over more than ten months, both exceeded the target advance distance and reached more than twice the life of the unmodified casting. After further reducing wall thickness and machining allowance, the service life was increased to more than three times the original. The rare-earth-modified precision casting process was then incorporated into normal production.
| Test unit | Total advance over trial period | Comparison with original |
|---|---|---|
| Modified casting 1 | 13,131.7 | More than twice the original life |
| Modified casting 2 | 10,675.7 | More than twice the original life |
My practical rules for shrinkage control in precision casting
From all of these experiences, I have developed a set of practical rules that I apply to every precision casting project. First, I confirm that the casting structure is suitable for precision casting. If the part was designed for another process, I redesign it to avoid isolated thick sections and abrupt transitions. Second, I identify all hot spots and feeding regions. Third, I design the gating system so that the last liquid is in the riser or sprue, not in the casting. Fourth, I verify the ingate size and position. Fifth, I select the pouring temperature and shell temperature to balance filling and feeding. Sixth, I improve local cooling where needed. Seventh, I use rare-earth modification or other alloy treatment when it improves fluidity and feeding. Eighth, I confirm the result by sectioning, mechanical testing, and field trials.
| Step | Action | Purpose in precision casting |
|---|---|---|
| 1 | Review casting structure | Avoid isolated hot spots and abrupt sections |
| 2 | Identify hot spots and feeding regions | Define where feed metal is needed |
| 3 | Design gating and riser | Move shrinkage out of the casting |
| 4 | Verify ingate size and position | Ensure feed path remains open |
| 5 | Set pouring and shell temperatures | Balance fluidity and directional solidification |
| 6 | Improve local cooling | Prevent corner and hot spot shrinkage |
| 7 | Use alloy treatment if needed | Increase fluidity and feeding ability |
| 8 | Validate by sectioning and testing | Confirm defect reduction and performance |
Conclusion
Shrinkage cavities and shrinkage porosity remain among the most important defects in precision casting. They form when the last liquid in a precision casting cannot be fed during liquid and solidification contraction. The main causes are poor gating design, unfavorable casting structure, high alloy contraction, improper pouring conditions, poor shell cooling, poor local heat dissipation, and insufficient pressure head. The main prevention method is directional solidification: the casting should freeze progressively toward the gating system, and the final shrinkage should be located in the riser or sprue. I achieve this through correct gating design, structural improvement, padding when necessary, controlled pouring, local cooling, adequate pressure head, and clean steel practice. When ordinary measures are not enough, rare-earth modification can improve fluidity and feeding, reduce porosity, and increase service life. In my experience, the most successful precision casting processes are those that combine careful thermal analysis, practical gating design, and repeated validation. Shrinkage control is not a single adjustment; it is a system of decisions that must be balanced against filling, stress, cost, and performance. When these decisions are made correctly, precision casting can deliver dense, reliable, and long-lasting components with far fewer shrinkage-related failures.