Research on a New Pouring System Process for Engine Cylinder Body Casting
Abstract This article focuses on the cylinder body casting of an 11-liter 6-cylinder engine of a commercial vehicle. By systematically
Abstract This article focuses on the cylinder body casting of an 11-liter 6-cylinder engine of a commercial vehicle. By systematically
Abstract:This article focuses on the cylinder block casting of an 11-liter 6-cylinder engine of a commercial vehicle. By systematically analyzing
After analyzing the defects, another improvement scheme is made, as shown in the figure. In the original scheme, the investment
Unreasonable pouring speed setting of investment casting will also produce insufficient pouring defects. In order to determine the reasonable pouring
Another investment casting thin-walled steel casting of ZHY casting was under poured in the trial production process, and the defects
In the casting defect scheme, the actual pouring temperature is 1560 ℃, and the actual average pouring speed is 0.38
The support size of a thin-walled steel casting is 400 mm × 310 mm × 270 mm, minimum wall thickness
Because the exhaust rib is not set in the original scheme, the simulation shows that the gas pressure in the
In recent years, with the application of advanced technologies such as high-performance (steel, non-ferrous alloy, etc.) materials, CAE analysis and