In the production of critical components for blast furnaces, the cooling wall stands out as a key element. This镶管 casting, which involves embedding steel pipes within the iron body, presents notable technical challenges in its manufacture. Traditional foundry methods such as green sand, resin sand, and sodium silicate sand casting have been commonly employed. However, an innovative shift towards using the lost foam casting process for these components has demonstrated significant advantages. This process not only meets stringent quality requirements but also offers superior economic and environmental benefits, including high sand reclamation rates, minimal solid waste generation, and enhanced production efficiency, aligning perfectly with the principles of a circular economy.
Technical Specifications for Blast Furnace Cooling Walls
The manufacturing of blast furnace cooling walls demands adherence to precise dimensional and performance criteria. The dimensional tolerances are typically defined as follows: thickness ±5 mm, height ±5 mm, inner and outer arc chord length ±3 mm. The bosses at the roots of the inlet/outlet cooling water pipes and around bolt holes must have a flat surface with a height tolerance of ±1.5 mm. The positional accuracy for the centers of all cooling water pipe openings is critical, with a tolerance of ±3 mm. After cleaning, each embedded pipe must undergo a pressure test, maintaining pressure for 10 minutes with a permissible pressure drop of ≤3% within 5 minutes. The embedded pipes are typically made from #10 steel, conforming to relevant standards. The required chemical composition and mechanical properties for the iron castings are summarized in the table below.
| Material Grade | C | Si | Mn | P | S | Tensile Strength (MPa) | Elongation (%) |
|---|---|---|---|---|---|---|---|
| HT200 | 3.2-3.5 | 1.6-2.2 | 0.6-0.9 | <0.20 | <0.150 | ≥200 | – |
| QT500-7 | 3.5-4.0 | ≤2.7 | ≤0.6 | ≤0.08 | ≤0.025 | ≥420 | ≥4 |
| QT400-18 | 3.4-4.0 | ≤2.8 | ≤0.5 | ≤0.07 | ≤0.030 | ≥370 | ≥12 |
The Lost Foam Casting Process Flow
The lost foam casting process is a precise sequence of operations that transforms a foam pattern into a solid metal casting. The core stages of this workflow are essential for achieving the desired quality in complex castings like cooling walls.
1. Pattern Making and Assembly
The process begins with the creation of a foam polystyrene (EPS) pattern, which is an exact replica of the final cooling wall, including all internal passages for the cooling pipes. These patterns are typically produced using pre-expanded beads in aluminum molds. The dimensional accuracy of this foam pattern is paramount, as it directly defines the cavity in the sand. The steel cooling pipes are carefully positioned and fixed within the foam assembly. A completed foam pattern ready for processing is a critical first step in the lost foam casting process.
2. Coating and Drying
The assembled foam pattern is then coated with a refractory ceramic slurry. This coating serves multiple vital functions: it provides a smooth surface finish on the final casting, enhances the pattern’s strength and rigidity to withstand sand compaction, and creates a barrier that prevents sand from penetrating the metal during pouring. After dipping, the coated pattern is transferred to a drying oven. Proper drying is crucial to remove all moisture; any residual water can lead to gas defects in the casting. The drying parameters (time and temperature) must be meticulously controlled based on the coating thickness and part geometry.
3. Molding and Compaction
The dried, coated patterns are placed into a vented flask. Dry, unbonded silica sand is then poured around the patterns while the flask is subjected to vibration. This vibration ensures the sand flows into all intricate details of the pattern and achieves a high, uniform packing density. A vacuum is applied to the flask to further rigidize the sand mass, creating a stable mold that can withstand the metallostatic pressure of the molten metal. The vacuum level is a key process parameter, typically controlled within a specific range:
$$ P_{vac} = 0.04 \text{ to } 0.06 \text{ MPa} $$
The exact value depends on the alloy; for gray iron it is often at the lower end (~0.04-0.05 MPa), while for ductile iron, a slightly higher vacuum (~0.05-0.06 MPa) is used to counter the greater expansion forces during solidification.
4. Melting, Treatment, and Pouring
Molten iron is prepared in a cupola or induction furnace to the target chemistry. For ductile iron grades, the melt undergoes a post-inoculation treatment. The common sandwich method is used: the magnesium-bearing nodulizing alloy is placed in a pocket at the bottom of a treatment ladle, covered with steel punchings or inert material. Approximately two-thirds of the required iron is poured into the ladne, initiating the vigorous reaction. After the reaction subsides, the remaining iron is added to dilute the melt, simultaneously introducing the inoculant. The inoculant addition varies by grade:
$$ W_{Inoculant(QT500-7)} \approx 0.4\% – 0.5\% $$
$$ W_{Inoculant(QT400-18)} \approx 0.7\% – 1.0\% $$
For the QT400-18 grade, an additional late stream inoculation of 0.2%-0.3% ferrosilicon is often performed for enhanced graphite nucleation.
The treated metal is then poured into the mold. The foam pattern vaporizes upon contact with the molten metal, and the metal front advances to take its shape. Pouring temperature is critically controlled:
$$ T_{pour(Gray Iron)} \approx 1290 – 1310^\circ\text{C} $$
$$ T_{pour(Ductile Iron)} \approx 1310 – 1320^\circ\text{C} $$
Maintaining the vacuum during and after pouring is essential for mold stability and for removing the gaseous products of foam decomposition.
5. Cooling, Shakeout, and Cleaning
After pouring, the casting is allowed to solidify and cool within the sand mold. Once sufficiently cool, the vacuum is released, and the sand, which is unbonded, flows freely away from the casting during shakeout. The high reusability of this dry sand (often >95%) is a major economic and environmental advantage of the lost foam casting process. The casting then undergoes shot blasting to remove any residual coating, followed by grinding to remove the gating system. The final and most critical step is the hydrostatic pressure test of the embedded cooling channels to ensure their integrity.

Production Results and Quality Control
Application of the described lost foam casting process yields cooling wall castings that consistently meet specification requirements. The table below presents typical chemical compositions and mechanical properties achieved in production, demonstrating compliance with the targets outlined earlier.
| Material Grade | C | Si | Mn | P | S | Mgres | REres | Tensile Strength (MPa) | Elongation (%) |
|---|---|---|---|---|---|---|---|---|---|
| HT200 | 3.44 | 1.83 | 0.64 | 0.083 | 0.044 | – | – | 206 | – |
| QT500-7 | 3.75 | 2.42 | 0.57 | 0.054 | 0.026 | 0.039 | 0.021 | 481 | 5.5 |
| QT400-18 | 3.59 | 2.67 | 0.43 | 0.049 | 0.028 | 0.051 | 0.032 | 440 | 13.9 |
Metallographic examination of ductile iron castings reveals a predominantly spherical graphite structure. The graphite nodularity and count are typically excellent, with grades often achieving a rating of 2-3 according to international standards (e.g., ISO 945), which is well within the acceptable range for the required mechanical properties. This confirms the effectiveness of the treatment and inoculation practices within the lost foam casting process.
Dimensional Analysis and Process Challenges
A detailed dimensional inspection of cooling walls produced via the lost foam casting process reveals distinct characteristics when compared to traditional sand casting methods.
Advantages: The dimensional accuracy of features such as the bosses at pipe roots and bolt holes is generally superior. This is because these features are directly formed by the precision-machined foam pattern, eliminating variability associated with core setting or mold erosion in conventional processes. Furthermore, the overall surface finish of the casting is significantly smoother and cleaner, owing to the refractory coating applied to the foam pattern.
Challenges: A recurring issue observed is minor dimensional deviation, particularly in the width of the casting. This deviation is more pronounced in ductile iron castings than in gray iron. The primary cause is attributed to the substantial graphite expansion during the eutectic solidification of ductile iron. This expansion can displace the un-bonded sand mold, leading to a slight increase in casting dimensions. The magnitude of this deviation, $\Delta D$, can be conceptually related to the expansion pressure, $P_{exp}$, and the compactability of the sand, $C_s$:
$$ \Delta D \propto \frac{P_{exp}}{C_s} $$
Where $P_{exp}$ is significantly higher for ductile iron than for gray iron.
Process mitigations to control this include stricter control of the sand compaction through optimized vibration parameters and maintaining the prescribed vacuum level to rigidize the mold. Additionally, a slight reduction in pouring temperature for ductile iron can be beneficial:
$$ T_{pour(QT)-optimized} \approx T_{pour(QT)} – \Delta T $$
where $\Delta T$ is a small reduction (e.g., 5-10°C) to reduce the total heat input and potentially moderate the expansion force, without compromising fluidity.
Economic Efficiency Comparison
The economic superiority of the lost foam casting process becomes evident when analyzing the cost structure, particularly for core-making and mold-making, compared to bonded sand processes. Consider a production batch of 20 cooling walls, each weighing 1.7 tons. The cost analysis below focuses on mold-making materials and pattern/tooling costs, excluding shared costs like melting and finishing.
1. Lost Foam Casting Process Cost ($C_{LFC}$):
The primary costs are the foam pattern and the labor for pattern assembly. The sand cost is negligible due to ~95% reclamation.
$$ C_{LFC} = N \times W \times (R_{foam} + R_{labor}) $$
Where:
$N$ = Number of castings (20)
$W$ = Weight per casting (1.7 tons)
$R_{foam}$ = Foam pattern cost per ton (e.g., $60/ton)
$R_{labor}$ = Pattern assembly labor cost per ton (e.g., $390/ton)
$$ C_{LFC} = 20 \times 1.7 \times (60 + 390) = \$15,300 $$
2. Resin Sand Process Cost ($C_{RS}$):
Costs include resin, catalyst, auxiliary materials (paint, seals), and a share of the wooden pattern cost.
$$ C_{RS} = [N \times W \times (U_{resin}P_{resin} + U_{cat}P_{cat} + C_{aux})] + \frac{C_{pattern}}{L_{pattern}} $$
Where:
$U_{resin}$, $U_{cat}$ = Usage of resin & catalyst (kg/ton) (e.g., 48 kg/t, 25 kg/t)
$P_{resin}$, $P_{cat}$ = Price of resin & catalyst ($/kg) (e.g., $13.5/kg, $4.0/kg)
$C_{aux}$ = Auxiliary material cost per ton (e.g., $45/ton)
$C_{pattern}$ = Wood pattern cost (e.g., $4,100)
$L_{pattern}$ = Pattern life in number of castings (e.g., 60)
$$ C_{RS} = [20 \times 1.7 \times (48 \times 13.5 + 25 \times 4 + 45)] + (4100 / 3) \approx \$28,329 $$
3. Sodium Silicate (CO2) Process Cost ($C_{SS}$):
Costs include new sand, sodium silicate binder, CO2 gas, auxiliary materials, and pattern share.
$$ C_{SS} = N \times W \times (U_{sand}P_{sand} + U_{silicate}P_{silicate} + C_{aux} + U_{CO2}P_{CO2}) + \frac{C_{pattern}}{L_{pattern}} $$
Where:
$U_{sand}$ = New sand usage (ton/ton casting) (e.g., 1.0 t/t)
$P_{sand}$ = Sand price ($/ton) (e.g., $200/ton)
$U_{silicate}$ = Silicate usage (kg/ton) (e.g., 90 kg/t)
$P_{silicate}$ = Silicate price ($/kg) (e.g., $3.8/kg)
$U_{CO2}$ = CO2 consumption (cylinders/ton) (e.g., 3 cylinders/t)
$P_{CO2}$ = CO2 price per cylinder (e.g., $23)
$$ C_{SS} = 20 \times 1.7 \times (1.0 \times 200 + 90 \times 3.8 + 45 + 3 \times 23) + (4100 / 3) \approx \$22,787 $$
The comparative analysis clearly shows that the lost foam casting process offers the lowest mold-making cost for this application ($15,300 vs. $28,329 and $22,787). The economic benefits are compounded by drastically reduced cleaning labor, as the castings require only shot blasting and minor grinding, bypassing the extensive knocking-out and core removal typical of bonded sand processes.
Conclusions
The implementation of the lost foam casting process for manufacturing blast furnace cooling walls has proven to be a technically viable and economically superior alternative to conventional sand casting methods.
1. The lost foam casting process consistently produces cooling wall castings that meet all chemical, mechanical, and pressure-test specifications. Its most significant advantages lie in its environmental and economic efficiency, characterized by extremely high sand reclamation (>95%), minimal solid waste generation, and streamlined production flow that reduces labor-intensive cleaning. This contributes substantially to sustainable foundry operations.
2. Dimensional accuracy on formed features like bosses and bolt holes is excellent due to the precision of the foam pattern. The overall surface finish quality of castings produced by the lost foam casting process is markedly superior to that achieved with traditional green or resin sand casting.
3. A key process challenge to manage is dimensional deviation, primarily in width, caused by the graphite expansion pressure during ductile iron solidification. This can be effectively controlled through stringent process parameter management, including optimizing sand compaction, maintaining correct vacuum levels, and fine-tuning pouring temperatures. The lost foam casting process, therefore, requires precise control but offers a highly rewarding solution for complex castings like cooling walls, with significant potential for broader application in heavy-section ductile iron castings.