Sand Casting Process Improvement of Water Pump Housing

In my work with sand casting parts, I have encountered numerous challenges related to shrinkage porosity and quality consistency. This paper describes my investigation into the sand casting process for a water pump housing used in an automotive engine cooling system. The housing has approximate dimensions of 240 × 200 × 150 mm, a single-piece weight of 5.4 kg, and an annual demand of about 20,000 pieces. The original production route relied heavily on empirical trial and error, which led to a shrinkage porosity rejection rate of about 20%. I decided to apply a systematic approach using three-dimensional modeling, numerical simulation, and controlled experiments to improve the casting quality of this particular sand casting part.

In the beginning, I analyzed the material requirements and the existing production workflow. The water pump housing is cast from grey cast iron, specifically a grade similar to HT250. The chemical composition of the base iron melt is summarized in Table 1. The mechanical properties of grey cast iron depend on the graphite morphology and the metallic matrix. Since the housing is a pressure-containing component, shrinkage porosity can directly lead to leakage during pressure testing. Therefore, controlling solidification is critical for obtaining sound sand casting parts.

Table 1: Base iron melt composition requirements for the water pump housing (mass fraction)
Element Range (%)
C 3.2 – 3.4
Si 1.6 – 1.8
Mn 0.8 – 1.1
P ≤ 0.10
S 0.05 – 0.12
Cr ≤ 0.25
Mo ≤ 0.15
Cu ≤ 0.50
Al ≤ 0.015
Ti ≤ 0.05
Sn ≤ 0.12
Pb ≤ 0.06

The production process for this sand casting part includes raw material inspection, weighing, melting in a medium-frequency induction furnace, sand preparation, molding with a jolt-squeeze molding machine, pouring on a linear conveyor, shakeout, fettling, shot blasting, and final inspection. The melting parameters are given in Table 2. Inoculation is performed during pouring using a barium silicon inoculant with a particle size of 2–10 mm. The chemical composition of the inoculant is shown in Table 3.

Table 2: Melting and pouring parameters
Parameter Value
Superheat temperature 1500–1550 °C
Superheat time 5–15 min
Chill test white width 5–10 mm
Tapping temperature 1470–1520 °C
Pouring temperature 1350–1420 °C
Pouring time per ladle 4–7 min
Table 3: Approximate composition of the inoculant used
Element Content (%)
Si 71.21
Ca 1.29
Al <1.2
Ba 3.79
Zr 2.16
Fe Balance

I first created a three-dimensional model of the water pump housing using Pro/E software. The main structural features include the inlet flow passage, guide vanes, volute chamber, tongue, throat, and the base or foot. The drawing also incorporates machining allowances and core prints. For sand casting parts, the design of the pattern and core boxes must account for shrinkage, draft, and dimensional tolerances. I set the dimensional tolerance grade as CT10 for this housing, since the molding process uses machine molding. The machining allowance was set to 2 mm on machined surfaces. The draft angle was chosen as 1.5°. The casting shrinkage rate for grey iron was taken as 0.9%. This means that the pattern dimensions are enlarged according to

$$K = \frac{L_{\text{mould}} – L_{\text{casting}}}{L_{\text{casting}}} \times 100\%$$

where \(K\) is the linear shrinkage rate, \(L_{\text{mould}}\) is the pattern dimension, and \(L_{\text{casting}}\) is the casting dimension. With \(K = 0.9\%\), the pattern dimensions are slightly larger than the final casting dimensions to compensate for contraction.

The pouring position and parting surface were determined based on the casting geometry and the need to place the most critical surfaces in the lower or vertical position. I chose a horizontal parting surface that splits the housing into an upper and lower half. A two-cavity mold was designed to improve productivity. The layout is shown conceptually in Figure 1. The pouring position and parting surface selection followed standard principles: important machined surfaces should face downward or sideways; heavy sections should be placed at the top to promote directional solidification; the number of cores should be minimized; and the parting surface should facilitate molding and core setting.

The design of the gating system is a critical factor for producing sound sand casting parts. I adopted a semi-closed gating system with a sprue, a runner, and two ingates. The ratios of the cross-sectional areas of the sprue, runner, and ingates were selected as 1.1 : 1.3 : 1.0. The minimum cross-sectional area of the resistance element (the ingate) was calculated using the Osann formula:

$$S_{\text{gate}} = \frac{m}{\rho \, \mu \, \tau \, \sqrt{2gH_{\text{avg}}}}$$

where \(m\) is the total mass of liquid metal flowing through the resistance section, \(\rho\) is the density of the liquid metal, \(\mu\) is the flow coefficient, \(\tau\) is the filling time, \(g\) is gravitational acceleration, and \(H_{\text{avg}}\) is the average metallostatic head. The volume of the casting was \(9.23 \times 10^5 \, \text{mm}^3\), and the mass was about 6.46 kg. I estimated the pouring mass as 9 kg, accounting for the gating system. The density was calculated as

$$\rho = \frac{m_0}{\nu} = \frac{6.46}{923} \approx 0.007 \, \text{kg/cm}^3$$

The flow coefficient \(\mu\) was taken as 0.50, and the filling time \(\tau\) was set to 15 seconds. The average static head was calculated from the geometry of the sprue and casting:

$$H_{\text{avg}} = H_0 – \frac{P^2}{2C}$$

with \(H_0 = 150 \, \text{mm}\), \(P = 95 \, \text{mm}\), and \(C = 127 \, \text{mm}\). This gives

$$H_{\text{avg}} = 150 – \frac{95^2}{2 \times 127} \approx 114.47 \, \text{mm}$$

Substituting these values into the Osann formula yields a total gate area of about 3.6 cm², i.e., 1.8 cm² per ingate. The runner area was 4.25 cm² (2.125 cm² each), and the sprue area was 3.27 cm². The detailed dimensions of the gating channels were as follows: ingate length 50 mm, width 12 mm at the bottom and 8 mm at the top, height 20 mm; runner length 100 mm, width 15 mm at the bottom and 10 mm at the top, height 17 mm; sprue diameter 20.4 mm, height 100 mm. The gating system was arranged to introduce the metal from the upper part near the thick sections of the housing. This promotes directional solidification, but it also creates a hot spot near the ingate, which was later identified as one of the sources of shrinkage porosity in sand casting parts.

To understand the solidification behavior and defect formation, I used the casting simulation software ProCAST. The simulation procedure involves several steps: creating the geometry, generating a finite element mesh, setting boundary conditions and material properties, running the filling and solidification analysis, and visualizing the results. The key governing equations for the filling process are the continuity, momentum, and energy equations. For an incompressible Newtonian fluid, the continuity equation is

$$\frac{\partial u}{\partial x} + \frac{\partial v}{\partial y} + \frac{\partial w}{\partial z} = 0$$

where \(u\), \(v\), and \(w\) are the velocity components in the \(x\), \(y\), and \(z\) directions. The momentum equations in the three directions can be written as

$$\frac{\partial u}{\partial t} + u\frac{\partial u}{\partial x} + v\frac{\partial u}{\partial y} + w\frac{\partial u}{\partial z} = -\frac{1}{\rho}\frac{\partial p}{\partial x} + g_x + \nu \nabla^2 u$$

$$\frac{\partial v}{\partial t} + u\frac{\partial v}{\partial x} + v\frac{\partial v}{\partial y} + w\frac{\partial v}{\partial z} = -\frac{1}{\rho}\frac{\partial p}{\partial y} + g_y + \nu \nabla^2 v$$

$$\frac{\partial w}{\partial t} + u\frac{\partial w}{\partial x} + v\frac{\partial w}{\partial y} + w\frac{\partial w}{\partial z} = -\frac{1}{\rho}\frac{\partial p}{\partial z} + g_z + \nu \nabla^2 w$$

where \(p\) is pressure, \(\rho\) is density, \(\nu\) is kinematic viscosity, and \(g_x, g_y, g_z\) are gravitational acceleration components. The energy equation is

$$\rho c_p \left( \frac{\partial T}{\partial t} + u\frac{\partial T}{\partial x} + v\frac{\partial T}{\partial y} + w\frac{\partial T}{\partial z} \right) = \nabla \cdot (k \nabla T) + S$$

where \(c_p\) is specific heat, \(T\) is temperature, \(k\) is thermal conductivity, and \(S\) is the heat source term due to latent heat release during solidification. The latent heat is modeled as

$$S = \rho L \frac{\partial f_s}{\partial t}$$

where \(L\) is the latent heat of fusion and \(f_s\) is the solid fraction. To track the free surface of the liquid metal, the volume of fluid (VOF) method is used. The volume fraction \(F\) is defined as

$$F = \frac{V_{\text{fluid}}}{V_{\text{cell}}}$$

where \(V_{\text{fluid}}\) is the volume of fluid in a cell and \(V_{\text{cell}}\) is the total cell volume. The evolution of \(F\) is governed by

$$\frac{\partial F}{\partial t} + u\frac{\partial F}{\partial x} + v\frac{\partial F}{\partial y} + w\frac{\partial F}{\partial z} = 0$$

For the solidification process, the Fourier heat conduction equation is solved together with the latent heat release. The equation is

$$\rho c_p \frac{\partial T}{\partial t} = \frac{\partial}{\partial x}\left(k \frac{\partial T}{\partial x}\right) + \frac{\partial}{\partial y}\left(k \frac{\partial T}{\partial y}\right) + \frac{\partial}{\partial z}\left(k \frac{\partial T}{\partial z}\right) + Q$$

where \(Q = \rho L \frac{\partial f_s}{\partial t}\) is the internal heat source. These equations are discretized using the finite element method in ProCAST.

In the simulation model, I used the material EN-GJL-250, which corresponds to HT250 grey cast iron. The mold material was defined as green sand, and the cores were made of phenolic resin-bonded sand. To simplify the calculation, all molding materials were treated as green sand. The initial temperature of the mold and cores was set to 25 °C. The pouring temperature was 1380 °C, and the pouring time was 15 seconds. The pouring was simulated as manual pouring, which in ProCAST means a prescribed time-varying flow rate or a fixed filling time. I used the fixed total filling time of 15 seconds.

The simulation results from the initial design showed that solidification begins at the thin edges of the flanges and at the lower curved pipe portion. The last region to solidify is the central part of the housing. More specifically, the simulations predicted that shrinkage porosity would likely form in three critical areas: the tongue (or septal tongue), the threaded connection at the upper part of the volute chamber (which is near the center of the casting), and the connection between the base and the volute chamber. These are the regions where isolated liquid pools form late in solidification because the surrounding metal has already solidified. Without sufficient liquid metal feed, these isolated pools contract and create porosity.

The root cause of the porosity was identified as an insufficiently sized riser and an improper solidification sequence. The original riser had a diameter of 40 mm and a height of 65 mm. It was located near the ingate, but its neck was too small, and it froze before the casting sections that needed feeding. Consequently, the liquid feed path was cut off early, leading to shrinkage porosity in the sand casting parts. Furthermore, the base area did not have any chilling or feeding devices, so it formed an isolated liquid region that could not be fed from any riser. The simulation indicated that the shrinkage porosity locations coincided with the defects observed in the actual production, as shown in Figure 2 (the figure is not reproduced here, but the locations were confirmed by sectioning and pressure testing).

To improve the casting quality, I proposed two main modifications: enlarging the riser and applying cooling coatings on the cores. For the riser at the center hole area, I changed its dimensions from 40 mm diameter × 65 mm height to 50 mm diameter × 80 mm height. This larger riser increases the module and the volume of available liquid metal, allowing the riser to stay liquid longer than the casting section it feeds. The modulus of a riser can be approximated by

$$M = \frac{V}{A}$$

where \(V\) is the volume and \(A\) is the heat-transferring surface area. For a cylindrical riser with diameter \(D\) and height \(H\), the modulus is

$$M = \frac{\pi D^2 H / 4}{\pi D^2 / 4 + \pi D H} = \frac{D H}{D + 4H / 4?}$$

Actually, for a cylinder with an open top, the bottom and side surfaces transfer heat; the top may be open or covered. If the top is insulated, the modulus is larger. The original riser had a smaller modulus and solidified prematurely. Increasing the diameter and height increases the modulus and feeding capacity. The modified riser provided sufficient feed metal to achieve directional solidification, with the riser as the last region to solidify.

For the isolated liquid region at the base, I designed a triangular chill. The dimensions of the chill were 65 mm, 40 mm, and 55 mm for the three sides, with a thickness of 32 mm. A chill helps to accelerate the cooling of a local hot spot, promoting simultaneous solidification and reducing the tendency for shrinkage porosity. The chill can be placed directly on the mold surface or, as in this case, simulated by applying a cooling coating to the corresponding area of the sand core. The cooling coating used was a zircon-based coating, which increases the heat extraction rate at the core surface. In the simulation, I modeled the effect of the cooling coating by modifying the interfacial heat transfer coefficient between the core and the casting in that region. The heat transfer coefficient was increased by a factor of about three to represent the enhanced cooling effect. This approach is often adopted for sand casting parts when a metal chill cannot be easily placed due to core geometry.

I also considered the design of the chill material. Common chill materials include copper, aluminum, cast iron, steel, graphite, and magnesia. Table 4 lists their thermophysical properties.

Table 4: Thermophysical properties of common chill materials
Material Density (kg/m³) Specific heat (J/(kg·°C)) Thermal conductivity (W/(m·°C)) Heat diffusivity (W·s^0.5/(m²·°C))
Copper 8930 385.2 392 3.67
Aluminum 2680 941.9 273.8 2.52
Cast iron 7200 669.9 37.2 1.34
Steel 7850 460.5 46.5 1.30
Synthetic graphite 1560 1356.5 112.8 1.55
Magnesia 3100 1088.6 3.5 0.344

The chill accelerates heat removal from the designated region, increasing the temperature gradient and facilitating directional solidification. It also refines the local microstructure by increasing the cooling rate, which is beneficial for the mechanical properties of sand casting parts.

After modifying the riser and adding the cooling/core coating, I reran the ProCAST simulation. The results showed a significant improvement in the solidification sequence. The larger riser remained molten until the end of solidification, providing continuous feed to the central hole region. The cooling coating on the core at the base region eliminated the isolated liquid pool, allowing that region to solidify concurrently with its surroundings. The shrinkage porosity indicators disappeared in both critical areas. The simulated temperature distribution at the end of filling and at several intermediate times confirmed that the temperature gradient was oriented toward the riser, and no closed liquid islands remained in the casting.

To verify the simulation results, I implemented the modified process in the foundry. The riser pattern was changed to the larger size, and the core at the base area was coated with a zircon-based cooling coating. I also maintained strict control over the chemical composition and pouring parameters to ensure reproducibility. The modified process was used to produce the water pump housing for a period of six months. The statistical results showed that the shrinkage porosity rejection rate dropped from 20% to less than 1%. Pressure tests showed no leakage caused by porosity. Visual and metallographic examinations confirmed that the defects were eliminated. The microstructure showed a more uniform distribution of graphite and a higher proportion of pearlite in the previously defective areas, comparable to other regions of the casting.

The improvement can be explained by the enhanced feeding efficiency of the riser and the modified cooling pattern. The modulus of the original riser can be compared with that of the casting section it feeds. For a cylindrical riser, the modulus is

$$M_{\text{riser}} = \frac{V}{A} = \frac{\pi D^2 H / 4}{\pi D^2 / 4 + \pi D H} \quad \text{(if top is open)}$$

Using \(D = 40 \, \text{mm}, H = 65 \, \text{mm}\):

$$M_{\text{riser}} = \frac{40 \times 65}{40 + 4 \times 65} = \frac{2600}{300} = 8.67 \, \text{mm}$$

For the modified riser, \(D = 50 \, \text{mm}, H = 80 \, \text{mm}\):

$$M_{\text{riser,new}} = \frac{50 \times 80}{50 + 4 \times 80} = \frac{4000}{370} = 10.81 \, \text{mm}$$

If the top of the riser is covered or insulated, the modulus is even larger. The increase from 8.67 mm to 10.81 mm represents about a 25% increase in modulus, which is typically sufficient to ensure that the riser outlasts the casting section. The feeding distance is also improved by adding the chill. The effective feeding distance of a riser can be expressed as

$$L_{\text{total}} = L_{\text{riser zone}} + L_{\text{end zone}}$$

The presence of a chill at the base region virtually extends the end zone, allowing the riser to feed a longer path. In this configuration, the center riser feeds the upper portion, while the cooled base region solidifies early and independently, avoiding the need for feeding from a distant source.

In conclusion, the numerical simulation using ProCAST was a valuable tool in diagnosing and solving shrinkage porosity in this water pump housing. The iterative process of simulating, modifying, and validating the process proved effective. The final process parameters and design changes are summarized in Table 5.

Table 5: Summary of process changes
Item Original Modified Effect
Riser diameter 40 mm 50 mm Increased feeding capacity
Riser height 65 mm 80 mm Increased modulus and feed time
Core coating at base None Zircon-based cooling coating Eliminated isolated liquid pool
Shrinkage porosity rate 20% <1% Improved pressure tightness

Through this study, I learned that the quality of sand casting parts can be substantially improved by combining computational simulation with careful engineering analysis. The ability to visualize the filling and solidification sequences allows the foundry engineer to identify hidden hot spots and optimize risers, chills, and gating systems before committing to expensive tooling changes. Moreover, the use of cooling coatings on cores is a practical and low-cost alternative to metal chills in complex internal cavities. This approach can be applied to similar sand casting parts where internal shrinkage porosity is a persistent problem.

For future work, I plan to extend this methodology to other components in the same product family. I will also investigate the effect of different pouring temperatures and cooling rates on the microstructure and mechanical properties of the gray iron. Furthermore, the use of inverse simulation to calibrate interfacial heat transfer coefficients from actual thermocouple data could improve the accuracy of the predictions. The continued development of digital casting simulation and process control will enable foundries to produce high-quality sand casting parts with minimal waste and maximum productivity.

In summary, the key conclusions from my research are:

  • The water pump housing, due to its uneven wall thickness and complex internal geometry, is prone to the formation of isolated liquid regions during solidification, leading to shrinkage porosity.
  • Enlarging the riser from 40 mm × 65 mm to 50 mm × 80 mm at the center hole location provides adequate feeding and establishes a favorable temperature gradient for directional solidification, eliminating porosity in that area.
  • The isolated liquid region at the base can be resolved by using a triangular chill with side lengths of 65 mm, 40 mm, and 55 mm and a thickness of 32 mm. In production, a zircon-based cooling coating applied to the sand core achieved the same effect.
  • After implementing these modifications, the shrinkage porosity rejection rate decreased from 20% to less than 1%, and no pressure-test failures were observed.

The findings demonstrate that numerical simulation is an essential tool for the modern foundry engineer. It transforms the traditional trial-and-error process into a rational engineering method. The improved process not only reduces defects but also shortens the development cycle and lowers production costs. I hope that the methodology and results presented here can serve as a reference for other engineers working on similar sand casting parts. By sharing this experience, I aim to promote the wider adoption of simulation-assisted design in the casting industry.

I believe that the combination of simulation, careful design, and process control will continue to drive the advancement of sand casting technology. The quality and reliability of sand casting parts will improve, opening new applications in automotive, hydraulic, and other engineering fields. My current results are specific to this water pump housing, but the same principles can be extended to other complex castings. The key is to understand the physics of heat transfer and fluid flow, to validate the simulation with experiments, and to implement robust process controls. In this way, the full potential of sand casting parts can be realized.

Scroll to Top