Rapid sand casting experiment of cylinder head
According to the design of sand core, riser and gating system, the general assembly drawing and explosion drawing of sand […]
According to the design of sand core, riser and gating system, the general assembly drawing and explosion drawing of sand […]
The reasonable gating system, riser, pouring temperature, pouring speed and other boundary conditions are optimized by using the criteria of
Through the research, a complete process route of rapid sand mold casting is obtained. ① ugnx8 0 software to establish
According to the analysis of sand casting process, the design of three gating systems is put forward. The influence of
According to the sand mold casting process CAD system developed by the laboratory, the casting process design is carried out.
With the development of economy, China’s automobile industry has developed rapidly, but it is facing the problems of unreasonable industrial
Ugnx8 0 software to model the three-dimensional model of sand casting engine cylinder head. UG NX is a new generation
The casting blank of automobile engine cylinder head produced by sand mold gravity casting is shown in Figure 2-1. ZL105
The engine is known as the “heart” of the automobile, and the cylinder head is one of the most important,
In the new era of the 21st century, China’s automobile industry is booming and has become a pillar industry of
1.Effect of aging treatment For the engine parts of gray cast iron cylinder head, such as cylinder block, cylinder head,
For a long time, the cylinder block and cylinder head have been made of gray cast iron. Due to the
The original material of zc170 cylinder head is HT300, the technical requirements are WCu = 0.5% ~ 0.8%, WCR =
1. Primary raw materials Q12 pig iron, industrial scrap, vermicularizing agent (wre = 9% – 11%, WMG = 4% –
Three kinds of annealing process were selected, and the annealing time was 18 h, 11 h and 8 h, respectively.
The structure of 11 l engine cylinder head casting is shown in Figure 1, and the overall dimension of the
Through the above analysis, the process was optimized: the furnace holding time was extended to about 8 h, the temperature
The structure of a 13 l cylinder head casting is shown in Figure 1, and the overall dimension of the
The residual stress of cylinder head castings has always been an important problem in cylinder head casting. After casting, due
With the economic development of the country, all walks of life are developing rapidly, and the machinery industry is also
The poor machinability is a common problem of Engine Castings in China, and it is also the biggest gap between
Leakage refers to the leakage phenomenon of the cylinder block (cylinder head) during the pressure test (water pressure / air
Modern engines have very strict requirements on cleanliness. For cylinder block (cylinder head) castings, only a few grams (g) of
Usually in the inner surface or hot spot of the casting, such as the water jacket cavity of the cylinder
Sand hole is also a common defect of cylinder block (cylinder head) casting, which is often found on the upper
Porosity is usually the most common defect in cylinder block castings, which often takes the first place in the scrap
With the rapid development of China’s automobile manufacturing industry, many high-end automobile brands have been launched almost at the same
The structure of cylinder block (cylinder head) casting is complex, and the wall thickness is quite different. The thick and
Throughout the development trend of engine technology at home and abroad, we are pursuing to reduce the wall thickness of