Sand inclusion defect of bolster and side frame steel castings
During the production of bolster and side frame by green sand casting, sand inclusion defects are found, which are mainly
During the production of bolster and side frame by green sand casting, sand inclusion defects are found, which are mainly
In 2014, ZHY Casting introduced a small lost foam casting production line, mainly for the development of castings for waste
① Molten steel smelting process Element C% Si% Mn% P% S% Cu% Range 0.10-0.28 0.20-0.45 0.30-0.68 ≤0.035 ≤0.035 ≤0.30 5T
In the field inspection, we should focus on the parts prone to casting defects. According to my experience in the
The weight of the steel casting of the motor shell is 381kg, which is similar to the barrel structure. The
In view of the serious casting defects in the small batch production process of ZHY Casting motor shell steel castings,
The formation mechanism and influencing factors of hot crack casting defects are very complex. So far, there are three main
The name of furan resin sand comes from furan no bake process in English. Furan resin sand casting is a
In 2020, the international and domestic economy went down seriously, the domestic foundry industry was in great depression, and many
The two kinds of MNS inclusion defects observed are formed on the surface of oxidized inclusions. According to the literature
Two different MNS inclusion defects were observed in cast steel. Fig. 1 shows the microscopic morphology of the first MNS
At present, the new technologies and methods to reduce the carburization of steel castings mainly include negative pressure combustion empty
The material studied is low alloy steel, and its main alloy elements are common elements such as C, Si, Mn,
Fig. 1 slag inclusion defect on the upper surface of medium and large steel castings after processing, which is visually
The non-metallic inclusions in molten steel during smelting and pouring are one of the important causes of cracks in steel
Slag inclusion casting defect refers to the casting defect formed by dry sand, coating and other inclusions as molten iron
Another investment casting thin-walled steel casting of ZHY casting was under poured in the trial production process, and the defects
Different from forged steel parts, steel castings for hull structure have low carbon content and good welding performance. Defective parts
Fig. 1 the visual characteristics of air hole defects on the upper surface of steel casting hub are round, the
In the casting defect scheme, the actual pouring temperature is 1560 ℃, and the actual average pouring speed is 0.38
1. Improvement measures 1.1 Inspection and control of molding sand performance While maintaining the original test items and requirements of
Bolster and side frame are important running parts on the bogie of rail freight car. They bear the gravity of
The measures and methods to reduce the carburization of lost foam casting steel castings mainly include the following aspects: (1)
The lost foam casting method is flexible and convenient in modeling and pouring, especially for products with complex structure. lost
According to the thinking method of formulating the inspection standard of JCSS hull steel castings in Japan, medium and large
Hot crack: the crack is an irregular curve, the inner surface is rough and black brown iron oxide. Cold crack:
The support size of a thin-walled steel casting is 400 mm × 310 mm × 270 mm, minimum wall thickness
In recent years, with the application of advanced technologies such as high-performance (steel, non-ferrous alloy, etc.) materials, CAE analysis and
According to the causes, the pores produced by lost foam casting steel castings are divided into the following four categories.
During the pouring process, due to the excessive amount of gas released by the thermal decomposition of the gas mold