Casting shrinkage defects in engine cylinder block and cylinder head
The structure of cylinder block (cylinder head) casting is complex, and the wall thickness is quite different. The thick and
The structure of cylinder block (cylinder head) casting is complex, and the wall thickness is quite different. The thick and
Features: After removing the riser, there is less meat in the neck of the riser. Causes: The shape and size
The shrinkage porosity and porosity are more common in ductile iron than in ordinary gray iron. To prevent them, more
Throughout the development trend of engine technology at home and abroad, we are pursuing to reduce the wall thickness of
Features: Invasive pore: the pore size is generally large, in the shape of round, ball or pear; the pear shaped
Die casting is a kind of metal mould pressure casting on die casting machine, which is the most efficient casting
6 Non metallic hard point (1) Features and inspection methods: In the process of machining or after machining, the appearance
Defect characteristics and detection methods A wormhole or loose hole appearing in the thick part of a casting or in
The bad spheroidization means that the spheroidization does not achieve the expected effect. The metallographic structure of poor spheroidization is:
Features: Shrinkage cavity: the hole with large volume, rough wall surface and irregular shape in the casting Shrinkage porosity: a
1.Deformation Long and plate castings are easy to deform. After some castings are processed, they will deform after a period
Metal mold casting is a modern technology of making hollow mold with heat-resistant alloy steel. The metal mold can be
1 Casting porosity (1) Features and inspection methods: After dissection, appearance inspection or flaw detection showed that the pores had
① Desulfurization treatment. The so-called desulfurization is to transfer the sulfur in the molten iron to the slag as much
Sand casting is a kind of traditional casting technology which takes sand as the main molding material to make the
1) Reasonable design of liquid lifting system Because the holding time is too long, or the liquid in the lifting
Defect characteristics and detection methods Fine wrinkles on the surface of casting or dark gray flakes peeling off from the
Features: A cavity or apparent lack of flesh containing sand particles on or within the surface of a casting Causes:
In the thick section of the casting, at the hot spot or the axis where the final solidification takes place,
Defect characteristics and detection methods There are gray white powder like spots or scabs on the thick parts of the
Features: During the molding operation, there is sand sticking on the formwork, and the mold cavity has such phenomena as
Inside, on or near the surface of the casting, there are smooth holes of different sizes, round, long and irregular
1.Porosity Casting defect characteristics Inside, on or near the surface of the casting, there are smooth holes with different sizes,
1) Identification of casting defects in sand casting Casting failure refers to the defect on the casting, incomplete outline shape,
1, Characteristics There are defects in some parts of the casting, which often appear in the thin-walled part, the farthest
1. EPC is suitable for the production of steel castings. Some measures can be taken to produce low carbon steel
Defect characteristics and detection methods It is an open hole or a dark hole embedded with molding materials on the
Various casting defects often occur in the production of steel castings. How to prevent these defects has always been the
1) Reasonable selection of casting alloy and casting structure. 2) Make reasonable technical requirements for castings (defects are allowed and
1.Porosity Features There are smooth holes of different sizes on the inner or surface of the casting. Main causes ①