Cause analysis of shrinkage porosity of nodular iron castings
Nodular cast iron solidifies in “paste”. Compared with gray cast iron, eutectic solidification time is long, the number of eutectic
Nodular cast iron solidifies in “paste”. Compared with gray cast iron, eutectic solidification time is long, the number of eutectic
The operation environment of wind turbine is relatively bad, and the supporting large parts should be used for a long
The fracture morphology of the failed nodular cast iron crankshaft shows the fracture process and mechanism of the nodular cast
In February 2021, an automobile company conducted a bench test and operated at full speed and full load for 65
After normalizing, the tensile strength and elongation of nodular cast iron are improved at 930 ℃. In nodular cast iron,
The tensile specimens of room temperature nodular cast iron as cast and treated at different normalizing temperatures were tested at
The samples as cast and normalized were observed by Kearns vh-5000 ultra depth of field optical metallographic microscope. The metallographic
Nodular cast iron is a spheroidal graphite cast iron obtained by spheroidization and inoculation. From the aspect of production, the
1. EPS foaming white mold EPS material has good cutting performance, fast NC machining speed and high precision. The mold
Lost foam casting process is a casting process in which EPS white mold models similar to the size and shape
Vacuum rim is a safety component of the driving system of transportation machinery such as commercial vehicles and engineering vehicles.
Nodular cast iron has high mechanical properties, good sand casting performance, good fluidity, no hot crack tendency, shrinkage and high
Production preparation shall be carried out according to the established scheme. Since the injector hole core is made of hot
The sand suction pump casting is mainly used for river dredging, dredging and Embankment Consolidation, and the delivery medium can
By controlling the size and distribution of graphite diameter and the spherical regularity of graphite, the correlation degree with the
Figure 1 (a) and figure 1 (b) show the hardness and strength changes of three groups of different samples respectively.
Fig. 1 shows the microstructure SEM of three groups of ductile iron samples. It can be seen from the figure
Nodular cast iron obtains spherical graphite through inoculation and spheroidization. Because the graphite is spherical, it is not easy to
Furan resin self hardening sand is used for molding and core making, and alcohol based zircon coating is used to
After the above WPS preparation, WPQR welding procedure qualification test shall be carried out to determine the WPS process reliability.
From 2015 to 2019, the wind power market was constantly changing and experienced two rush loading peaks of wind power.
Based on all the previous analysis, the fracture process of nodular cast iron crankshaft is as follows: in the induction
Casting refers to pouring molten metal into the mold, cooling and forming to form a casting that meets the relevant
As shown in Figure 1, cut the metallographic sample close to the crack source, and then conduct rough grinding, fine
In recent years, with the development of mechanical equipment towards portability, low energy consumption and high efficiency, new requirements are
1. Defect analysis (1) The inner cavity of the cylinder body is a long strip-shaped sand core, and the gas
1. Defect analysis (1) The slag cleaning treatment of molten iron is not complete; (2) The results show that the
1. Defect analysis (1) There is a great difference in the wall thickness between the cylinder body and the shaft
1. Defect analysis (1) The stiffness of the base frame of the model is not enough, and the model is
The casting is molded in a box of 2 pieces, with 550 kg spheroidizing treatment package, 10 boxes and 3