Design principle of feeding system for sand casting of mud pump body
After determining the geometric characteristics, modulus and other parameters of sand castings, the feeding system can be designed. The following […]
After determining the geometric characteristics, modulus and other parameters of sand castings, the feeding system can be designed. The following […]
Ultrasonic flaw detection can only qualitatively analyze casting defects, but can not accurately describe defects. There are many scanning blind
1.Detect defects The probe specified by the supplier and the buyer shall be used to scan the inspection area of
The formation mechanism of hot tears casting defects mainly includes liquid film theory and strength theory. According to the liquid
Mesh generation is the basis of numerical simulation. At present, there are two main methods of division, namely, finite difference
In terms of experimental research on weld performance of cast steel joints, Zou Hui of Southeast University conducted fatigue tests
The new sand process scheme of sand mold casting and the reclaimed sand plus new sand process scheme pour 8
During the solidification process of sand casting, the volume of steel castings will shrink, and shrinkage porosity, shrinkage cavity and
According to the constancy of sound velocity propagation in the same medium and the proportional relationship between propagation distance and
The appearance characteristics of hot tears casting defects are that the tears propagates along the grain boundary, the appearance is
The samples for nondestructive testing are 24 cast steel joints randomly selected from the cast steel joints of civil engineering
It can be seen from the simulation results that the pouring system of the mud pump body of sand casting
The causes of cracks and sand inclusion defects in motor shell steel castings are studied from the perspective of process
Cast steel joints will inevitably produce some defects in the production process, such as hot crack, shrinkage cavity, delamination, slag
Scheme I The casting mud pump body adopts single bag and single hole pouring, and the diameter of the injection
The research on the mechanical properties of cast steel itself includes the research on the mechanical properties of cast steel
① Sand casting process scheme The sand casting process scheme adopts the top pouring system. All the workpieces are in
Ultrasonic flaw detection mainly detects the near surface and internal quality of steel castings, and the internal quality of steel
With the development of spatial structure, the span of structure is becoming larger and larger, and the forms are also
Due to the differences in product structure, weight, process equipment of production enterprises, production conditions and process technology level, there
Ester hardened sodium silicate self hardening sand process is a new generation of self hardening sand process developed on the
The crack and sand inclusion of motor shell steel castings are the inertia quality problems in casting production, and they
The formation reason and process of tensile crack casting defect are different from that of shrinkage crack casting defect. 1)
From April to December 2020, ZHY casting fully applied the optimized new sand mold casting process to production, and produced
From January to March 2020, ZHY Casting used the above process to produce 200 motor housings in small quantities. Basically,
The pouring process of sand casting is a very important link in the whole casting process. Usually, many foundries regard
It is necessary to establish an effective three-dimensional model when using ProCAST to analyze the filling process of sand casting
When designing the structure of sand castings, we should not only consider the requirements of mechanical properties and working performance,
The mud pump body of sand casting is made of ZG35, which belongs to medium carbon cast steel, with high
Crack casting defect is the biggest obstacle restricting the popularization and application of furan resin sand process in steel castings.