Control of other elements in ductile iron
(1) Composition control and selection of as Cast Ferritic Nodular Iron: Micro hypereutectic composition, in which the carbon is slightly […]
(1) Composition control and selection of as Cast Ferritic Nodular Iron: Micro hypereutectic composition, in which the carbon is slightly […]
It is recommended that the optimum spheroidizing temperature range is 1420-1480 ℃, the spheroidizing temperature of nodular cast iron is
Through research and production practice, the following key problems must be solved in order to produce high-quality and mass qualified
1. Design of formwork thickness The following contents shall be considered in the design of formwork: (1) the mold shell
The top pouring system of sand mold casting for tractor box adopts rain pouring, which is divided into four oval
Since the development and popularization of the process of producing crankshaft with iron film coated sand in the 1970s, due
① Increase the diameter of ladle nozzle and the size of gating system; ② Increase the number of ladle nozzles;
Although the application of shell casting in China is more than ten years later than that in foreign countries, it
The shell mold casting process of S1100 single cylinder diesel engine crankshaft was studied. S1100 single cylinder diesel engine crankshaft
Company profile: The Foundry Branch of Shanghai Diesel Engine Co., Ltd., located at No. 2636, Jungong Road, Shanghai, is a
Therefore, we analyze and sort out the causes of sand sticking in cast wear-resistant low alloy steel and the preventive
In 1940, Johannes Croning, a German engineer, invented the thermal method for manufacturing shell mold, which is called “C” method
The production of crankshaft blank by wet mold sand process is still the main traditional casting process, while the representative
A new type of cylinder block EA888 is a high-end sand casting. Due to its complex structure and wall thickness
There are many problems to be solved in the valve casting process, and relevant personnel should focus on the following
The weight of tractor box castings is 205KG, and the estimated gating system mass is 20kg. According to the manual,
The choke cross-sectional area, i.e. the cross-sectional area of the ingate, is designed according to the choke section method. After
The gating system of tractor box castings generally includes sprue cup, sprue, runner and inner sprue. Whether the gating system
The selected tractor reducer case is a large-scale casting designed by a company, which is produced in large quantities. It
Crankshaft is not only the main key transmission part of engine, but also an important safety part. When the engine
(1) Super duplex stainless steel SAF2507 has good chloride stress corrosion resistance under low stress. Generally, 18-8 austenitic stainless steel
The pouring temperature of cast iron is generally controlled between 1360 ℃ and 1450 ℃. In this paper, the pouring
SAF2507 is the third generation of super duplex stainless steel, American Standard (national standard ZG 00Cr25Ni7Mo4N). Its microstructure has an
Experts and scholars at home and abroad have studied the application of numerical simulation technology in the fields of sand
(1) The simulation flow of numerical simulation software is introduced, and the setting of simulation parameters of reducer box body
The so-called pressure casting mainly refers to the aluminum alloy wheel hub casting obtained by filling the liquid metal into
How to overcome the shortcomings of quartz sand and significantly reduce the sand holes and pores of large and medium-sized
As shown in Figure 1, it shows the filling flow state and temperature distribution at different times when the intermediate
In the casting forming of tractor box, if the parameters are set improperly, such as the mold cavity is too
Company profile: Dongfeng Automobile Co., Ltd. Foundry Branch is located at No. 1, Checheng Avenue, Xiangfan City, Hubei Province, covering