Problems in Casting Process of Ductile Iron for Testing Machine Nut
1. Analysis of cavity layout process The ductile iron casting process (see Figure) is divided from one end. All the
1. Analysis of cavity layout process The ductile iron casting process (see Figure) is divided from one end. All the
Figure 1 shows the location of shrinkage porosity in a casting. See Figure 2 for the process plan before improvement.
At present, the nut of testing machine produced by our company is easy to produce shrinkage cavity and porosity defects,
In recent years, there have been several innovations in grey cast iron production aimed at improving both quality and efficiency.
The sand casting surface obtained from the test is complete, but shrinkage cavities are found at the bearing holes of
According to the casting structure and sand casting process, the metal mold for the box and cover is designed. The
A. Cost problem: Although the as-cast high-performance ductile iron has less heat treatment than ADI castings, and has certain economic
In mechanical products with relatively small load but light weight requirements, aluminum alloy gearbox is a good choice. The problems
The casting simulation software was used to simulate the mold filling and solidification process of the balance shaft support. Figure
According to the comprehensive evaluation results of typical sand casting processes, for the static pressure casting process and V method
Sand casting has different types such as wet sand casting process and non clay sand casting process. The static pressure
The diesel engine structure for combat vehicles is V-shaped and symmetrical, and the left and right cylinder head castings are
Based on the above sand casting process analysis, there are many kinds of materials involved in the sand casting production
Sand casting is a kind of molding method that molten metal into flowing liquid alloy, then burned into the sand
It is found that only a small amount of shrinkage porosity occurs at the inner runner when observing the inside
(1) Ductile iron castings have large overall dimensions, high requirements for size and wall thickness control, large wall thickness difference,
(1) The casting process plan determines that the casting adopts the whole sample sand box molding production mode. According to
First of all, it is necessary to conduct solid modeling and mesh division, and then set parameters. This is the
Shrinkage cavity and shrinkage porosity are common defects in sand casting production. The main purpose of numerical simulation of sand
In order to analyze the stress and deformation of casting diaphragms before and after repair welding, a three-dimensional solid model
(1) Ductile iron samples with silicon content of 2.9%~4.6% were prepared by EPC process, and the matrix structure was ferrite.
Decarburization is the loss of carbon from the surface or near-surface layers of a material during heat treatment. It can
The upper surface of the steel casting is easy to produce defects such as sand holes, air holes and slag
In recent years, Austempered ductile iron (ADI, CADI) has made great progress in the selection of grinding ball materials due
Cast grinding ball is a kind of wear-resistant product with a large amount of applications in nonferrous metal and metallurgical
1. Sand casting structure and technical requirements The sand mold casting of the end cover is shown in Figure 1.
Three wear-resistant pump body castings were poured in production, and three attached cast test blocks were taken. The numbers of
1. Spheroidization Select the spheroidizing method of the dam type spheroidizing ladle rushing method, select the mixed rare earth spheroidizing
During the use of the wear-resistant pump body casting, the high-density hard particles move close to the cavity wall, thereby