Sand casting and precision casting process plan of nuclear power valve
In order to stabilize the casting process quality, there are strict regulations on the casting process, material, process and quality
In order to stabilize the casting process quality, there are strict regulations on the casting process, material, process and quality
The yellow area is the coating part. The first step in the yellow area is to mix the coating, and
Leakage refers to the leakage phenomenon of the cylinder block (cylinder head) during the pressure test (water pressure / air
In order to increase the local cooling speed of the casting, the metal block placed in the cavity and the
For the role of cold iron in the anti shrinkage process of castings, the sequential solidification theory and the equilibrium
Shrinkage defects will reduce the elongation of the material, and have a great impact on the load-bearing performance, impact resistance
EPC is divided into white area, yellow area and black area, and each part is closely linked and highly related.
Riser is a cavity used to store liquid metal in the mold. It supplies metal when the casting is formed,
The strength of casting coating can not be divided into two situations: one is the normal drying strength, the other
In the past, riser design basically followed the principle of sequential solidification, which needs to meet the following three conditions:
This type of beam is one of the main parts of a large machine tool. The quality of the casting
Shrinkage cavity and porosity are inevitable defects in a kind of die casting wheel. In the microstructure, the shrinkage cavity
The anode steel claw for electrolytic aluminum is also called electrolytic claw. There are parallel three claws, four claws, three-dimensional
Modern engines have very strict requirements on cleanliness. For cylinder block (cylinder head) castings, only a few grams (g) of
Ingot mold is a kind of necessary ingot equipment used in mold casting production in steel plant. Although its shape
The use of riser is one of the basic means to solve the shrinkage of casting. Although there are new
1) The reasonable design of the riser, the heat preservation sleeve and the casting pouring system constitute the riser system,
Calculation of resistance cross section The total sectional area a can be calculated according to the following formula =Q/KTL in
Defect characteristics and detection methods It is often found after sand cleaning or sand blasting of castings that the layered
In the casting of automobile parts, the wheel casting is a little different. Because it needs to meet a series
For the convenience of research, the pouring system is classified into top pouring, bottom pouring and step pouring according to
The pouring system is a channel to guide liquid metal into the mold cavity, which is composed of sprue cup,
Features: The appearance of the casting is incomplete, with a crack like gap or broken flow, and the metal edge
At present, there are many researches on the influence of metallurgical and molding factors on shrinkage cavity and porosity of
Due to the use of lightweight aluminum alloy materials, compared with the steel and cast iron used before, automatic production
Because the equipment is the core platform for the implementation of the technology, and the composite squeeze casting method is
The function of sand core is to form the inner cavity, hole of casting and the part that can’t produce
Sand inclusion refers to that there is a layer of metal lump or sheet on the surface of the casting,
7 Discoloration and spots (1) characteristics: There are different colors and spots on the casting surface. (2) Causes: ① Improper
1. Definition of composite squeeze casting Direct squeeze casting technology pressure directly acts on the surface of liquid metal, the