Detection and analysis of cracking failure test of casting support plate
The support plate is a part of the truck suspension part, also known as the support arm, connecting plate, etc.
The support plate is a part of the truck suspension part, also known as the support arm, connecting plate, etc.
In order to ensure the performance of turbocharger shell at 1050 ℃, a high nickel (20wt%) austenitic steel ASTM HK40
The increase in length of high silicon molybdenum ductile iron when it is cooled to room temperature after holding for
Although the amount of magnesium used in automobile industry is increasing, its application in automobile is still limited. At present,
1 Preliminary test As the pores are non fissured, N2 pores are excluded. In order to reduce the source of
The relationship between length increment and holding time of high nickel ductile iron at different operating temperatures is shown in
1. Defect category identification According to the shape and location of the stoma, the defect was initially identified as subcutaneous
Automotive exhaust is mainly composed of CO, CH and NOX. It directly discharges into the air not only pollutes the
The red oxide layer of high nickel ductile iron covers the surface of the sample while holding for 80 hours
1. Production process The 693 brake caliper and 812 brake caliper of ZHY casting are produced in the same line,
Fig. 1 shows the microstructure of high silicon molybdenum ductile iron after different thermal cycles at the upper temperature of
Before molding, assemble the core box according to the requirements, pay attention to the assembly sequence and the positioning of
With the continuous progress of society, atmospheric warming and environmental pollution have attracted more and more attention around the world.
Subcutaneous porosity is a common casting defect of nodular iron castings. The moisture in molding sand, resin in sand core,
Alloy cast iron is an iron-carbon cast alloy with some other elements added. It is often made by melting some
The as-cast microstructure of high nickel ductile iron observed under a microscope is shown in the figure.The graphite spheroidization of
1.Analysis of the reasons for the failure of the original process 1.1 cause analysis of shrinkage and porosity The riser
The figure shows the original as-cast structure of high silicon-molybdenum ductile iron. From Figure a, it can be seen that
The structure of the material determines the performance of the material, and the matrix structure of the material is often
By controlling chemical composition, optimizing and improving the spheroidizing incubation process, the graphite grade and size of QT450-10 can be
At present, the majority of machine tool castings are still gray cast iron. The practice at home and abroad has
With the improvement of performance requirements of automobile parts for ductile iron parts, its material brand and performance exceed the
The traditional method of high strength gray iron is to reduce the eutectic degree, to increase the austenite content and
1. Characteristics of inoculation treatment Up to now, there is no agreement on the mechanism of inoculation treatment at home
Al-Si series alloy is the most widely used alloy system with the most varieties in cast aluminum alloy, and there
The chemical composition of grey cast iron is composed of two parts: one is the basic composition, i.e. the five
Advantages of 3D printing technology in sand casting The emergence of 3D printing technology has certain advantages in additive manufacturing.
Foundry has long been a big polluter of environment. Not only foundry workers have been working in the harsh environment
The control system of vacuum differential pressure casting is one of the key factors to ensure the quality of castings,
In the high temperature compression test of Al Si based casting materials, the samples have compression deformation under different temperature