Optimization objective function of characteristic parameters of Sand Mold casting process Design
The process parameters related to the characteristics of sand casting process design are taken as the optimization object, and the
The process parameters related to the characteristics of sand casting process design are taken as the optimization object, and the
In order to effectively analyze the comprehensive benefits of carbon emission, production time and resource cost of foundry enterprises, the
At present, some scholars divide resource costs into energy, material and labor costs. According to the research boundary of sand
The production time is calculated from the melting of sand mold casting production stage to the stages of modeling, core
The microhardness of the machined surface was measured by MH- 6 microhardness tester. During the test, the pressure load was
The measured chemical composition of the experimental material is obtained by chemical analysis method and meets The measured chemical composition
The surface roughness is measured by using the TR200 handheld roughness meter of Beijing Times Instruments, and the roughness is
At the end of the experiment, the machined surface of the workpiece was observed by Keynes laser microscope (VK-X200K). In
The blade used in the experiment is monolithic PCBN and the binder is A1. Figure 1 shows the energy spectrum
In the process of cutting, the heat in the cutting area gradually accumulates at the arc of the tool tip,
PCBN cutters can be used for rough machining to improve machining efficiency, or finish machining to improve surface quality. This
The source of cutting force is the resistance of the tool to overcome elastic deformation, plastic deformation and friction. The
The experiment was carried out in the DAEWOOACE-V500 vertical machining center. The schematic diagram of orthogonal milling is shown in
In orthogonal turning, only one straight cutting edge is involved in the cutting, and the cutting edge is perpendicular to
There are many commonly used constitutive equations of metallic materials, including Power-Law model, Zerilli-Arstrong model, Johnson-Cook model and so on.
1. Data processing of tensile experiment. Figure 1 shows the stress-strain curve of static tensile test. As can be seen
Figure 1 shows the small Hopkinson pressure bar equipment used in this experiment. Figure 2 is a schematic diagram of
Because the chromium white cast iron used in the experiment is brittle material and has not been heat treated, the
Impact toughness is an important index of large wear-resistant plate. It refers to the ability of material to absorb plastic
It can be seen from Figure 1 that compared with the normal pressure, the hardness of the alloy can be
Different from equilibrium solidification, the solidification process of alloy melt under pressure is controlled by nucleation and subsequent crystal growth.
It has been proved that different types of carbides have different hardness. The purpose of different casting processes is to
Besides discussing the interface structure, which is the mechanism of atom stacking and crystal morphology, we also need to discuss
Crystal growth is a process in which the atoms in the liquid phase migrate and stack to the surface of
From the point of view of thermodynamics, primary carbides should only exist in hypereutectic alloy. But in fact, it can
Because the composition of low chromium white cast iron alloy 1 is far away from eutectic point, the carbides are
In the solidification process of Hypoeutectic chromium white cast iron, the primary phase is austenite, the carbides in the solidification
The total amount of carbides, eutectic carbides and primary carbides in alloy 2 are shown in the figure. The content
In order to better compare the solidification structures of different sampling positions under different pressures, the solidification structures of top,
(1) Solidification structure of specimens at different positions under atmospheric pressure The solidification structure of alloy 2 under normal pressure