Casting and heat treatment of ductile iron piston
Ductile iron piston is mainly used in medium speed diesel engine. It is the key component of diesel engine. It
Ductile iron piston is mainly used in medium speed diesel engine. It is the key component of diesel engine. It
Normalizing ductile iron piston Normalizing, also known as normalizing, is to heat the workpiece to Ac3 or Accm above 30~50
The wall thickness of ductile iron piston varies greatly, the thinnest part is 7.5 mm, the thickest part is 23
The casting properties of ductile iron have the following characteristics ① The content of sulfide and oxide in molten iron
The solidification process of ductile iron castings is generally a process of shrinkage, expansion and re shrinkage. Although the precipitation
Nodular cast iron (ductile iron for short) is the 50th century A kind of high strength cast iron developed in
The design of feeding system is the key content of this paper. We discussed the main factors that affect the
The surface of high nickel ductile iron samples during corrosion process was observed. The results are similar to that of
By observing the surface of the sample during the corrosion process, no obvious bubbles were found on the surface of
The unit area gain of high nickel ductile iron at 900 C for different working hours is recorded in Figure
The prepared sample is heated in a resistance furnace and weighed with an electronic balance.Figure 1 shows the measurement results
In order to understand the oxidation conditions at the cracks, elemental analyses are carried out on the areas of Fig.
The sample size for thermal fatigue test is 15 mm x 10 mm x 10 mm.To eliminate the influence of
The temperature range of the thermal cycle (T) is equal to the upper limit temperature of the thermal cycle (T)
During the extensive use of Ferritic Ductile iron, nickel is often added to improve its heat resistance. When the content
Ductile iron with ferrite matrix has certain strength, good impact toughness and plasticity, which can be obtained as-cast or by
In the 1940s, some scientific workers found that adding Ce, Mg and other elements into FERROCARBON alloys and nickel-carbon alloys
The increase in length of high silicon molybdenum ductile iron when it is cooled to room temperature after holding for
The relationship between length increment and holding time of high nickel ductile iron at different operating temperatures is shown in
Although the macroscopic changes of the ductile iron studied are not obvious, the corrosion surface is slightly uneven after enlarged
Automotive exhaust is mainly composed of CO, CH and NOX. It directly discharges into the air not only pollutes the
The red oxide layer of high nickel ductile iron covers the surface of the sample while holding for 80 hours
Fig. 1 shows the microstructure of high silicon molybdenum ductile iron after different thermal cycles at the upper temperature of
With the continuous progress of society, atmospheric warming and environmental pollution have attracted more and more attention around the world.
Alloy cast iron is an iron-carbon cast alloy with some other elements added. It is often made by melting some
Ductile iron is commonly used to make structural parts on mechanical parts and equipment, mainly due to its relatively low
The as-cast microstructure of high nickel ductile iron observed under a microscope is shown in the figure.The graphite spheroidization of
1.Analysis of the reasons for the failure of the original process 1.1 cause analysis of shrinkage and porosity The riser
The figure shows the original as-cast structure of high silicon-molybdenum ductile iron. From Figure a, it can be seen that
The composition of slag inclusions is mainly composed of magnesium silicate, oxide, sulfide and sulfur oxide, which is a very